Chapter 19

Material and Hardness Testing

A steel bar’s certificate lists numbers such as Re 360, Rm 520, A 26%, KV 45 J, and 160 HB. Where do these numbers come from? They come from laboratory tests conducted on workpieces of the material, according to standards that are the same worldwide. In this chapter, we’ll look at which properties are important to designers and fabricators, what a metal looks like on the inside, and then each test individually: tensile testing with all its calculations, compression and bending tests, impact testing with a pendulum, Brinell, Vickers, and Rockwell hardness tests, fatigue testing, and non-destructive testing methods that detect defects without breaking the workpiece. By the end, we’ll know how to read a certificate and select a material based on its specifications.

19.1 Properties of Materials

Choosing a material means asking yourself what the workpiece needs to do: support a load, withstand impacts, resist wear, be easy to machine, be weldable, and be lightweight. Each of these requirements corresponds to a property of the material, and almost every property has its own test. These properties are divided into four categories.

  • Mechanics: how materials react to forces. Strength, elasticity, ductility, toughness, hardness, and fatigue resistance. These are the main topics of this chapter.
  • Physical properties: density, melting point, thermal expansion, thermal and electrical conductivity, and magnetic behavior. These properties do not vary much from one type of steel to another, but they vary greatly among different material families (steel, aluminum, plastic).
  • Technological Properties: how the material can be processed into a finished workpiece. Machinability, weldability, hardenability, cold formability (bending, deep drawing), and castability in foundries.
  • Chemical properties: particularly resistance to corrosion and oxidation at high temperatures.
PropertiesWhat does it say?How is it measured?
ResistanceHow much load can it withstand before it becomes permanently deformed or breaks?Tensile strength: Re, Rm (N/mm²)
Elasticity and Stiffnesshow much it deforms under load and then returns to its original shapemodule of elasticity E (N/mm²)
Ductilityhow much it stretches and deforms before breakingElongation A% and reduction Z%, bending tests
Tenacityhow much energy it absorbs before breaking, especially during impactsCharpy impact test: KV (J)
Hardnesshow resistant it is to penetration and, in practice, to wear and tearBrinell, Vickers, and Rockwell tests
Fatigue StrengthHow long can it withstand a load that goes back and forth millions of times?fatigue test, Wöhler curve
WorkabilityIf the cut is done correctly: chips, tool wear, finishingComparative cutting tests (Chapter 24)
Weldabilityif it can be welded without cracks or brittle areaschemical composition (carbon equivalent), joint testing
Hardenabilityhow much depth the hardening has during quenchingJominy test (heat treatments: Chapter 22)

Be careful with two words that are often confused. Hard does not mean tough: glass is extremely hard but breaks with a single blow; copper is soft but does not break. And durable does not mean rigid: quenched and tempered steel can withstand three times the load of structural steel, but under the same load (as long as it remains elastic), it deforms exactly like structural steel, because the module of elasticity (E) is the same (Section 10.4).

Weldability and Carbon Equivalent

The more carbon and alloying elements a steel contains, the more difficult it is to weld: near the weld bead, the metal heats up and then cools quickly, and if the steel is highly hardenable, a hard and brittle zone forms there that can crack. To get a quick idea, we calculate the carbon equivalent, which adds the other elements—weighted according to their effect—to the carbon content.

Carbon Equivalent (International Institute of Welding formula)
CE = C + Mn6 + Cr + Mo + V5 + Ni + Cu15
Each chemical symbol represents the mass percentage of the element (as indicated on the casting certificate). CE up to approximately 0.40–0.45: good weldability; above this, preheating and a controlled procedure are required; above approximately 0.6, welding is difficult. These are approximate thresholds.
Example 19.1 · Three Types of Steel for Welding

Typical compositions: S355 with 0.18% C and 1.40% Mn; C45 with 0.45% C and 0.65% Mn; 42CrMo4 with 0.42% C, 0.75% Mn, 1.05% Cr, and 0.22% Mo. Other elements are negligible.

S355: CE = 0.18 + 1.40 / 6 = 0.18 + 0.233 = 0.413
C45: CE = 0.45 + 0.65 / 6 = 0.45 + 0.108 = 0.558
42CrMo4: CE = 0.42 + 0.75 / 6 + (1.05 + 0.22) / 5 = 0.42 + 0.125 + 0.254 = 0.799
S355 welds without any problems; C45 requires preheating; 42CrMo4 can only be welded using a specially designed procedure

19.2 What a Metal Looks Like on the Inside

To understand why a metal stretches, why it hardens when hammered, or why it becomes brittle in the cold, you have to look at it very closely. The atoms in a solid metal are not arranged randomly as they are in a liquid: they are arranged in regular files, repeated in all three directions, and form a crystal lattice. The smallest unit that, when repeated, makes up the entire lattice is called a unit cell. Almost all metals used in engineering have one of these three unit cells.

CCC · body-centered cubicα-iron (ferrite), Cr, Mo, WCFC · face-centered cubicγ-iron (austenite), Al, Cu, NiEC · hexagonal close-packedtitanium, magnesium, zinc
Figure 19.1 · The three most common unit cells. The atoms at the vertices are shown in blue; those at the center of the cube (CCC), at the center of the faces (CFC), or in the midplane of the prism (EC) are shown in red.
  • Body-centered cubic (BCC): one atom at each corner of the cube and one at the center. This structure is found in iron at room temperature (α-iron, ferrite), chromium, molybdenum, and tungsten. These are strong metals, but they can become brittle at low temperatures.
  • Face-centered cubic (FCC): one atom at each vertex and one at the center of each face. This structure is found in aluminum, copper, nickel, iron above 912 °C (γ-iron, austenite), and austenitic stainless steels such as AISI 304. They have many planes along which atoms can slide: they are very ductile and remain tough even at extremely low temperatures.
  • Compact hexagonal (EC): a prism with a hexagonal base. Titanium, magnesium, and zinc have this structure at room temperature. They have few slip planes and are more resistant to cold deformation.

Iron changes its crystal structure with temperature: it is CCC up to 912 °C, CFC between 912 and 1394 °C, and CCC again until it melts at 1538 °C. This change, known as allotropy, is the reason why steel can be hardened: we will discuss this in Chapters 20 and 22.

Grains

As molten metal cools, crystals begin to grow simultaneously at many points, each with files of atoms oriented in its own way, until they touch one another. A workpiece of metal is therefore made up of millions of tiny crystals—called grains—ranging in size from a few thousandths to a few tenths of a millimeter, separated by grain boundaries. These can be seen under a microscope after the workpiece has been polished and etched with a mild acid. Useful rule: a fine grain produces a stronger and more ductile material, because the grain boundaries hinder the movement of atoms and halt the propagation of cracks. A workpiece heated for too long, on the other hand, causes the grain to coarsen and becomes brittle.

Alloys

Pure metals are rarely used on their own: other elements are almost always added, resulting in an alloy. The added atoms can replace those of the base metal (solid-state substitution, such as nickel in copper or chromium in iron), and slip into the spaces between the atoms (interstitial solution, such as carbon in iron), or form a new, hard, and brittle compound with the base metal (such as cementite, Fe3C in steels). In all cases, the foreign atoms disrupt the lattice and make sliding more difficult; this is why an alloy is almost always stronger than the pure metal.

🔬
Plastic deformation and work hardening. When a metal undergoes permanent deformation, entire planes of atoms slide over one another—not all at once, but one step at a time—due to defects in the crystal lattice called dislocations. During cold deformation, dislocations multiply and interfere with one another, and the metal becomes harder and less ductile: this is work hardening—what happens to a copper wire bent back and forth—and what we will observe in the middle section of the tensile test.

19.3 Tensile Test: Test Specimen and Testing Machine

The tensile test is the most important of all: a single test provides the strength, ductility, and module of elasticity. It is performed on a test specimen cut from the material, which is slowly pulled until it breaks while a machine records the force and elongation. The rules for testing metals are established by the UNI EN ISO 6892-1 standard.

The Test Tube

The test specimen has two thicker ends, which fit into the machine’s clamps, and a thinner, calibrated section of constant cross-section, connected to the ends with wide radii to prevent fracture at the fillets. It can be round (turned from a bar) or flat (cut from a sheet of metal). Two reference marks are made on the calibrated section at a distance L0: this is the initial length between the marks, over which the elongation will be measured.

gripping headgripping headreference marksd₀L₀ = 5.65 · √S₀Lc (calibrated section)Lt (total length)duLu (after breakage)after breakage, with the two workpieces rejoined:
Figure 19.2 · Round tensile test specimen. Above, before the test, with diameter d₀ and the three lengths; below, the two workpieces brought back together after fracture: the notches have moved apart by a distance of Lu, and at the point of fracture, the diameter has decreased to du.

Elongation at break depends on the shape of the test specimen: a stubby specimen elongates by a greater percentage than a long one, because the final constriction exerts a greater force on a short length. To obtain comparable results, proportional test specimens are used, in which L0 is related to the cross-sectional area by a fixed ratio.

Proportional test tube
L0 = 5,65 · √S0 round-bottom test tube: S0 = π · d0²4 → L0 ≈ 5 · d0
L0: initial length between the reference points in mm · S0: initial cross-sectional area of the calibrated section in mm² · d0: initial diameter in mm. The coefficient 5.65 applies to the “short” test specimen, which is the most commonly used; there is also a long test specimen with a coefficient of 11.3 (L0 ≈ 10 · d0). The standard requires L0 to be at least 15 mm.
Example 19.2 · The length between the reference points

Calculate L0 for a round test specimen with a diameter of 10 mm and for a flat test specimen measuring 20 × 5 mm.

Circular: S0 = π · 10² / 4 = 78.54 mm²; √78.54 = 8.862 mm
L0 = 5.65 × 8.862 = 50.07 mm → rounded to 50 mm (i.e., 5 times the diameter)
flat: S0 = 20 × 5 = 100 mm²; L0 = 5.65 × √100 = 5.65 × 10 = 56.5 mm
L₀ = 50 mm for the Ø10 round bar, 56.5 mm for the 20 × 5 flat bar

The car

The universal testing machine has a very rigid frame with a fixed crosshead and a movable crosshead, driven by two ball screws (or by a hydraulic cylinder in larger machines). The test specimen is clamped between two wedge-type grips. A load cell—a transducer that measures force—is located between the crosshead and the upper grip; an extensometer, which attaches directly to the calibrated section, measures elongation to the nearest thousandth of a millimeter. The crosshead moves slowly, at speeds specified by the standard, and a computer records everything and draws the curve in real time.

load cell (F measurement)top clampingextensometer (measurement ΔL)lower gripmovable crossbarscrew(or hydraulic)(lowers smoothly)test tube
Figure 19.3 · Universal testing machine, schematic diagram. The movable crosshead moves downward, causing the specimen to elongate; the load cell measures the force, and the extensometer measures the elongation of the section between the reference points.

19.4 The Test Diagram and Its Parameters

The machine draws the load-elongation diagram: force F in kN on the vertical axis, and elongation ΔL in mm on the horizontal axis. However, this diagram depends on the dimensions of the test specimen: a larger specimen can withstand more force. To obtain the material’s “identity card,” divide the force by the initial cross-sectional area and the elongation by the initial length: this yields the stress-strain diagram σ-ε, which has the same shape but applies to any test specimen made of that material.

From Load to Stress
σ = FS0 ε = ΔLL0 ε% = ΔLL0 · 100
σ: conventional stress (tension) in N/mm² · F: force in N · S0: initial cross-sectional area in mm² · ε: strain (unit elongation), pure number · ΔL: elongation in mm · L0: initial length between the reference points in mm. It is called “conventional” because it is always divided by the initial cross-sectional area, even when the test specimen has already been thinned.
10020030040051015202530σ (N/mm²)ε (%)elasticyieldwork hardeningneckingfractureA = 26.4%ReH = 247ReL = 237Rm = 402slope = E
Figure 19.4 · σ-ε diagram from the test in Example 19.5 (S235 steel). The elastic region is drawn much wider than it actually is: in reality, it ends at 0.11% and would be indistinguishable from the vertical axis. After fracture, the elastic portion is recovered (dashed line), and the permanent elongation A remains.

The Four Zones

  • Elastic region. The stress increases in proportion to the strain (Hooke’s law, σ = E · ε): the stress-strain curve is a straight line, and its slope is the module of elasticity E. When the load is removed, the specimen returns to its original length.
  • Yielding. In mild steels, once a certain stress is reached, the material yields suddenly: the force drops slightly and then fluctuates as the test specimen elongates by a few percent without the need for additional load. The peak value before yielding is the upper yield strength ReH; the lowest value during creep, excluding the initial drop, is the lower yield strength ReL. In calculations, ReH is usually used as the value guaranteed by the material standard; ReL is more reproducible from one test to another. From this point onward, the deformations are largely permanent.
  • Work hardening. The material becomes stronger as it deforms, and the stress rises to its maximum value, the unit breaking load Rm (tensile strength). In this region, the test specimen elongates and tapers uniformly along its entire calibrated length.
  • Constriction. After reaching its maximum, the deformation is concentrated at a single point; the cross-section there narrows like a bottleneck, the required force decreases, and the test specimen breaks.

The unit deviation load Rp0.2

Many materials do not have a distinct yield point: quenched and tempered steels, stainless steels, aluminum alloys, and copper alloys transition from the elastic region to the plastic region along a smooth curve. Instead of Re We use the unit load of deviation from proportionality Rp0,2: the force at which the unloaded test specimen would remain elongated by 0,2% permanently. It is found on the diagram by drawing a straight line parallel to the elastic region starting at ε = 0.2%: the point where it intersects the curve gives Rp0,2. In the R material tablese e Rp0,2 They are used in the same way—as a limit that should not be exceeded.

1002003004005006007000.20.40.60.81.01.2σ (N/mm²)ε (%)Rp0.2 ≈ 490 N/mm²Rm = 700 N/mm², reached later (around 7%)a straight line parallel to the elastic region,shifted by 0.2%
Figure 19.5 · Beginning of the stress-strain curve for a heat-treated C45 steel (Example 19.3): no yield step. The blue line, parallel to the elastic region and shifted by 0.2%, intersects the curve at Rp0.2 ≈ 490 N/mm².

Test Parameters

Resistance
ReH = FeHS0 ReL = FeLS0 Rp0.2 = Fp0.2S0 Rm = FmS0
FeH, FeL: upper and lower yield strengths in N; Fp0.2: force causing 0.2% permanent deformation in N; Fm: maximum test force in N; S0: initial cross-sectional area in mm². All results are in N/mm² (MPa).
Ductility and stiffness
A% = Lu − L0L0 · 100 Z% = S0 − SuS0 · 100 E = ΔσΔε
A%: percentage elongation after fracture · Lu: distance between the reference points measured on the rejoined workpieces, in mm · Z%: percentage reduction in area · Su: minimum cross-sectional area after fracture, in mm² (for round bars: π · du² / 4) · E: module of elasticity in N/mm², slope of the linear portion · Δσ and Δε: changes in stress and strain between two points in the elastic region.

The elongation A% is permanent: the small elastic portion disappears when the test specimen breaks. If the test specimen is not proportionally short, the length used is written next to A: A11.3 for the long test specimen, A80mm for the thin sheets tested with L0 = 80 mm. Values based on different reference lengths cannot be compared with one another.

Example 19.3 · A steel with no yield point: quenched and tempered C45

8-mm-diameter test specimen made of quenched and tempered C45 steel. From the diagram, with a 0.2% yield strength: Fp0.2 = 24.6 kN; maximum force Fm = 35.2 kN. After fracture, the marks are 45.6 mm apart.

S0 = π · 8² / 4 = 50.27 mm²; L0 = 5.65 · √50.27 = 40.06 mm → 40 mm
Rp0.2 = 24,600 / 50.27 = 489.4 N/mm²
Rm = 35,200 / 50.27 = 700.3 N/mm²
A% = (45,6 − 40) / 40 · 100 = 14,0%
Rp0.2 ≈ 490 N/mm², Rm ≈ 700 N/mm², A = 14%: typical values for quenched and tempered C45 steel
Example 19.4 · Stretching and Shrinking Stainless Steel

A Ø10 AISI 304 test specimen with L0 = 50 mm has Lu = 72.5 mm and a minimum diameter of du = 5.6 mm after fracture.

A% = (72,5 − 50) / 50 · 100 = 45,0%
Su = π · 5.6² / 4 = 24.63 mm²; S0 = 78.54 mm²
Z% = (78,54 − 24,63) / 78,54 · 100 = 68,6%
A = 45%, Z ≈ 69%: Austenitic stainless steel is very ductile and can be deep-drawn and bent easily

19.5 Complete Example of a Tensile Test

Let's put it all together using data from a test on a round bar of structural steel. The numbers are made up, but they're the ones you'd actually see in a test report for S235.

Measured valueValue
initial diameter d0 (average of three measurements taken with a micrometer)10.00 mm
length between reference points L050.0 mm
a point on the elastic region, measured with the extensometerF = 10.0 kN with ΔL = 0.0303 mm
Upper yield strength FeH19.4 kN
Lower yield strength FeL18.6 kN
maximum force Fm31.6 kN
distance between the reference points after the Lu break63.2 mm
minimum diameter in the fracture zone du6.1 mm
Example 19.5 · All results from a test on S235
initial cross-sectional area: S0 = π · 10² / 4 = 78.54 mm² (proportional test piece: 5.65 · √78.54 = 50.07 ≈ 50 mm ✓)
module of elasticity: σ = 10,000 / 78.54 = 127.32 N/mm²; ε = 0.0303 / 50 = 0.000606
E = σ / ε = 127.32 / 0.000606 = 210,106 N/mm² ≈ 210,000 N/mm²
Upper yield strength: ReH = 19,400 / 78.54 = 247.0 N/mm²
lower yield strength: ReL = 18,600 / 78.54 = 236.8 N/mm²
tensile strength: Rm = 31,600 / 78.54 = 402.3 N/mm²
Elongation: A% = (63.2 − 50) / 50 × 100 = 13.2 / 50 × 100 = 26.4%
Calculation: Su = π · 6.1² / 4 = 29.22 mm²; Z% = (78.54 − 29.22) / 78.54 · 100 = 62.8%
yield ratio: ReL / Rm = 236.8 / 402.3 = 0.59
E ≈ 210,000 N/mm², ReH = 247, ReL ≈ 237, Rm ≈ 402 N/mm², A = 26.4%, Z ≈ 63%: a S235 that meets specifications (ReH ≥ 235, Rm between 360 and 510)

A few observations on the results. Yield occurs with a very small elastic strain: ε = 236.8 / 210,000 = 0.113%, meaning that the 50-mm-long test specimen elongated by just 0.056 mm before yielding, while at fracture it elongated by 13.2 mm. The yield ratio Re/Rm indicates the margin between the first sign of yielding and fracture: in mild steels, it is approximately 0.6; in quenched and tempered steels, it rises to 0.7–0.9. A low ratio is a guarantee: the workpiece deforms noticeably before breaking, causing notice.

🛠️
The module of elasticity (E) is not measured using the crosshead. The crosshead’s displacement also includes the settlement of the grips and the elasticity of the machine: this is acceptable for A%, but not for E, which requires an extensometer on the calibrated section. If a “crosshead” diagram yields a steel with E = 80,000 N/mm², it is not the steel that is unusual—it is the measurement.

19.6 Compression Test and Bending Test

Compression

The compression test crushes a short cylinder (with a height one to three times its diameter, so that it does not bend at the tip) between two parallel plates. It is used primarily for brittle materials that perform well under compression but poorly under tension: cast iron, concrete, stone, ceramics, and some plastics. A ductile material such as mild steel, on the other hand, does not break: it bulges outward and becomes increasingly flattened, so the test yields only the compressive yield strength, which is approximately equal to the tensile yield strength. Gray cast iron fractures along a tilted plane of approximately 45°, where the shear stress is greatest.

Bend

In the three-point bending test, a bar rests on two rollers separated by a distance L and is loaded at the center. The maximum bending moment under the load is F · L / 4 (Section 10.8). This test is used for brittle materials (cast iron, cemented carbide, ceramics, glass, reinforced plastics), which are difficult to grip for a tensile test without breaking them at the ends. The result—the flexural strength—is always higher than the tensile breaking load of the same brittle material, because only the outermost fibers reach the maximum stress.

FFcast iron: it breaksalong a planeinclinedCompressionFLM max = F · L / 4Bending on three supports
Figure 19.6 · On the left, the compression test: the cast iron breaks along a tilted plane. On the right, bending on three supports, with the maximum moment occurring under the load.
Compressive and Flexural Strength (Round Test Specimen)
σc = FS0 σf = MW = F · L / 4π · d³ / 32 = 8 · F · Lπ · d³
σc compressive strength and σf flexural strength in N/mm² · F breaking force in N · S0 initial cross-sectional area in mm² · M maximum bending moment in N·mm · W flexural module in mm³ (Section 10.9) · L distance between supports in mm · d bar diameter in mm
Example 19.6 · A small cast-iron cylinder under the press

A small cylinder made of EN-GJL-250 gray cast iron, with a diameter of 20 mm and a height of 30 mm, fails under compression at 280 kN. Compare this with the tensile strength Rm ≈ 250 N/mm².

S0 = π · 20² / 4 = 314.16 mm²
σc = 280,000 / 314.16 = 891.3 N/mm²
ratio: 891.3 / 250 = 3.57
σc ≈ 890 N/mm²: Under compression, cast iron is more than three and a half times as strong as it is under tension.
Example 19.7 · Deflection of a Cast-Iron Rod

A Ø30 mm bar made of the same cast iron, supported at intervals of 300 mm, breaks in the middle under a load of 15 kN.

M = F · L / 4 = 15,000 · 300 / 4 = 1,125,000 N·mm
W = π · 30³ / 32 = 2,650.7 mm³
σf = 1,125,000 / 2,650.7 = 424.4 N/mm²
σf ≈ 424 N/mm², about 1.7 times the tensile strength: for a brittle material, these two values are not interchangeable

19.7 The Charpy Impact Test

The tensile test is a slow process: the force increases gradually. But many workpieces are subjected to impact, and certain materials that are ductile under slow loading shatter like glass when struck, especially in cold temperatures and if there is a notch. The impact test measures precisely this: how much energy the material absorbs when it breaks suddenly. It is performed using the Charpy pendulum (UNI EN ISO 148-1 standard).

The test specimen is a bar measuring 10 × 10 × 55 mm with a V-notch 2 mm deep, at a 45° angle, and with a bottom radius of 0.25 mm. It rests on two anvils with the notch facing away from the impact. A heavy hammer, mounted on an arm that rotates around a pivot, is raised to a fixed height and released: at its lowest point, it strikes the test specimen, breaks it, and continues rising on the other side. If the test specimen had absorbed no energy, the hammer would rebound to the same height; the energy expended to break it is the difference between the initial and final potential energy. A pointer on the dial, driven by the hammer, directly indicates this value in joules.

h₁h₂αβpinRhammer at the startafter breakagetest specimen on the supports, at the lowest point
Figure 19.7 · The Charpy pendulum. The hammer starts at height h₁ (angle α), breaks the test specimen at its lowest point, and rises only as high as h₂ (angle β): the difference in potential energy is the absorbed energy KV.
Energy absorbed in the Charpy test
KV = m · g · (h1 − h2) h = R · (1 − cos α) KV = m · g · R · (cos β − cos α)
KV: energy absorbed by the V-notch, in J · m: mass of the hammerhead in kg (essentially the reduced mass at the center of impact) · g = 9.81 m/s² · h1, h2 initial and final heights in m · R distance between the pivot and the center of the hammer in m · α initial angle and β final angle, measured downward from the vertical. Friction and air resistance are neglected; the machine compensates for these during an empty-load test.
Example 19.8 · Energy from heights

The hammer has a mass of 20 kg and is dropped from a height of 1.50 m. After breaking an S235 test specimen, it rebounds to a height of 0.95 m.

Initial energy: E0 = 20 × 9.81 × 1.50 = 294.3 J (it is a 300 J pendulum)
residual energy: E1 = 20 × 9.81 × 0.95 = 186.4 J
KV = 294.3 − 186.4 = 20 × 9.81 × (1.50 − 0.95) = 107.9 J
KV ≈ 108 J: well above the 27 J required by the standard for S235JR at 20 °C
Example 19.9 · Energy from Angles

A pendulum with a 20-kg mass at a distance R = 0.80 m from the pivot, with an initial angle of α = 150°. After breaking free, the pendulum swings back up to an angle of β = 95°.

cos 150° = −0.8660; cos 95° = −0.0872
h1 = 0,80 · (1 + 0,8660) = 1,4928 m ; h2 = 0,80 · (1 + 0,0872) = 0,8697 m
KV = 20 · 9.81 · 0.80 · (−0.0872 + 0.8660) = 156.96 · 0.7788 = 122.2 J
KV ≈ 122 J (out of a total available energy of 20 × 9.81 × 1.4928 = 292.9 J)

The transition temperature

Structural steels (CCC lattice) exhibit different behavior depending on temperature. At high temperatures, they fracture ductilely: the fracture surface is dull and fibrous, the material deforms significantly, and it absorbs a great deal of energy. At low temperatures, fracture becomes brittle: the surface is shiny and granular, with almost no deformation and very few joules absorbed. The transition occurs within a narrow range, known as the ductile-brittle transition zone. By conducting tests at different temperatures, the transition curve is plotted: a steel is suitable if, at all operating temperatures, it lies in the upper part of the curve. CFC metals (aluminum, copper, austenitic stainless steel) do not undergo this transition and are also used for liquefied gas tanks.

supportsupportmalletV-notch2 mm, 45°551010 × 10 mm cross-section, top view−80−4004050100150KV (J)T (°C)27 Jbrittleductiletransition
Figure 19.8 · On the left, the Charpy test specimen with the V-notch on the support side and the impact on the opposite face. On the right, a transition curve typical of S355J2 steel: the required 27 J is exceeded down to approximately −36 °C.

For this reason, the designation for structural steels includes the letters indicating the guaranteed toughness: JR means at least 27 J at +20 °C, J0 means 27 J at 0 °C, and J2 means 27 J at −20 °C (Chapter 20). A crane operating outdoors in the mountains is not built using JR steel. In the past, impact strength was also expressed in J/cm², calculated by dividing by the cross-sectional area beneath the notch (0.8 cm²); today, only the energy in joules is specified.

19.8 Hardness and the Brinell Test

Hardness is the resistance a material offers to penetration by a harder object. Hardness tests are the most commonly used in workshops because they are quick, inexpensive, and leave only a small indentation on the workpiece: they can be performed on the finished part, for example, to verify that a heat treatment was successful. They all work the same way: an indenter of a known shape is pressed into the material with a known force, and the size or depth of the indentation is measured. The smaller the indentation, the harder the material.

The Brinell Test

In the Brinell test (UNI EN ISO 6506-1), a carbide ball with a diameter of D (10, 5, 2.5, or 1 mm) is pressed into the material with a force F for 10–15 seconds. Once the load is removed, two perpendicular diameters of the indentation are measured under a microscope, and their average is calculated as d. The hardness is the force divided by the area of the spherical cap left by the ball.

DFdhcarbide balld₁d₂d = (d₁ + d₂) / 2the indentation as seen under a microscope
Figure 19.9 · Brinell test. On the left, the sphere with diameter D leaves an indentation with diameter d and depth h (ratio d/D = 0.42, as in Example 19.10). On the right, the indentation viewed from above: two diameters are measured at 90°.
Brinell Hardness
HBW = 0.102 · 2 · Fπ · D · (D − √(D² − d²)) F = 9,807 · k · D²
HBW Brinell hardness (the "W" stands for tungsten carbide ball; it is often written simply as HB) · F test force in N · D ball diameter in mm · d average indentation diameter in mm · k load factor, the ratio 0.102 · F / D², selected according to the material. The factor 0.102 = 1/9.807 converts the result back to the old kilogram-force units: thus, the numbers remain the same as always.

To ensure that tests conducted with different balls yield the same result, the load must be selected in proportion to D²: the load factor k is determined based on the material. Furthermore, the indentation must be between 0.24 · D and 0.6 · D: if it is smaller or larger, the measurement is invalid, and the load must be adjusted. The workpiece must be at least 8 times as thick as the depth of the indentation, and the indentations must be spaced away from the edges and from one another.

Materialload factor k = 0.102 · F / D²where D = 10 mm: F
steel, cast iron, nickel and titanium alloys3029,420 N (3,000 kgf)
copper alloys (brass, bronze), aluminum alloys for machining operations109807 N (1000 kgf)
pure aluminum and soft alloys54903 N (500 kgf)
very soft metals (tin, lead)1981 N (100 kgf)

These are illustrative and simplified examples; the standard provides the complete table based on the expected hardness range.

The result is expressed using the test conditions: 207 HBW 10/3000 means a hardness of 207, a 10-mm ball, and a load of 3,000 kgf (29,420 N). The Brinell test is used up to about 650 HBW; the large indentation makes it suitable for non-homogeneous materials such as cast iron, because it averages across many grains, but it is not suitable for thin workpieces, hardened surfaces, and finished parts where the indentation would be a problem.

Example 19.10 · Brinell hardness test on steel

Ball D = 10 mm, F = 29,420 N. The two measured diameters are 4.18 and 4.22 mm.

d = (4.18 + 4.22) / 2 = 4.20 mm; check: 4.20 / 10 = 0.42, between 0.24 and 0.6 ✓
√(10² − 4,20²) = √(100 − 17,64) = √82.36 = 9.0752 mm
D − 9.0752 = 0.9248 mm (the depth is half that: h = 0.462 mm)
HBW = 0.102 × 2 × 29,420 / (π × 10 × 0.9248) = 6,001.7 / 29.053 = 206.6
207 HBW 10/3000: This is the hardness of quenched and tempered C45 steel
Example 19.11 · Brinell Test on an Aluminum Alloy

A 5-mm ball with a load rating of k = 10 is used on a 6082-T6 aluminum sheet. The indentation measures 1.85 mm on average.

F = 9.807 × 10 × 5² = 2,452 N (250 kgf)
check: 1.85 / 5 = 0.37 ✓ ; √(25 − 1,85²) = √21.578 = 4.6452 mm
HBW = 0.102 · 2 · 2452 / (π · 5 · (5 − 4.6452)) = 500.2 / 5.573 = 89.7
90 HBW 5/250

19.9 The Vickers Test and Microhardness

In the Vickers test (UNI EN ISO 6507-1), the indenter is a diamond pyramid with a square base, with an angle of 136° between opposite faces. The indentation is a square when viewed from above: the two diagonals, d1 and d2, are measured, and their average is calculated. As with the Brinell test, hardness is the force divided by the area of the indentation, and the calculation results in a very simple formula.

F136thdiamond pyramidwith a square basedepth ≈ d / 7d₁d₂d = (d₁ + d₂) / 2the two diagonals of the footprint
Figure 19.10 · Vickers test. On the left, the pyramid with a 136° angle between its faces sinks by about one-seventh of its diagonal. On the right, the square indentation with the two diagonals to be measured.
Vickers Hardness
HV = 0.1891 · Fd² d = d1 + d22
HV = Vickers hardness · F = test force in N · d = average of the diagonals in mm · d1, d2 = measured diagonals in mm. The number 0.1891 = 0.102 × 2 × sin 68° comes from the geometry of the pyramid and the standard conversion to kilogram-force.

The great advantage of the Vickers test is that the shape of the indentation does not change with the load: the same number is obtained regardless of the force applied, and a single scale covers everything from lead to hard metal. The load is selected based on the thickness and hardness of the workpiece and is written after the designation: HV30 means a load of 30 kgf (294.2 N), HV10 is 98.07 N, and HV1 is 9.807 N. The workpiece must be at least 1.5 times as thick as the diagonal, and the surface must be smooth, because the diagonals are measured under a microscope.

Example 19.12 · Vickers HV30 on steel

Load F = 294.2 N (HV30). The diagonals measure 0.452 and 0.458 mm.

d = (0.452 + 0.458) / 2 = 0.455 mm; d² = 0.207025 mm²
HV = 0.1891 × 294.2 / 0.207025 = 55.63 / 0.207025 = 268.7
depth of the indentation: approximately 0.455 / 7 = 0.065 mm
269 HV30

Microhardness

With very small loads, ranging from 0.01 to 1 kgf (0.098 to 9.8 N), the Vickers test becomes a microhardness test: the indentations are only a few hundredths of a millimeter in size and are made on polished specimens, with the indenter’s placement determined under a microscope. It is used to measure the hardness of a thin layer (case-hardened, nitrided, chrome-plated), a single grain, or a welded area, or to trace the hardness profile from the surface toward the core of a treated workpiece. The elongated Knoop pyramid is also used; it leaves a narrow, shallow indentation, making it suitable for very thin layers.

Example 19.13 · Microhardness on a nitrided layer

An HV0.5 test (0.5 kgf = 4.903 N) is performed on a nitrided shaft. The average diagonal length is 0.0352 mm.

d² = 0.0352² = 0.00123904 mm²
HV = 0.1891 × 4.903 / 0.00123904 = 748.3
depth ≈ 0.0352 / 7 = 0.005 mm, or 5 µm: the nitrided layer, which is a few tenths of a millimeter thick, is not penetrated
748 HV0.5: typical of a nitrided layer

19.10 The Rockwell Test and Portable Hardness Testers

The Brinell and Vickers methods require measuring the indentation under a microscope. The Rockwell test (UNI EN ISO 6508-1), on the other hand, measures the depth of the indentation, and the hardness tester displays the reading directly on the dial or screen in just a few seconds. This is why it is the most commonly used test in workshops and heat treatment departments.

The test is conducted in three stages. First, a preload F0 = 98.07 N (10 kgf), which causes the penetrator to sink slightly and overcome surface irregularities: this position becomes the reference zero. Then the additional load F1 for a few seconds, and the indenter sinks deeper. Finally, the system returns to preload only: part of the deformation—the elastic portion—is recovered, and the instrument measures the permanent depth e relative to zero. Every 0.002 mm of depth is worth one Rockwell point; the number is read “backwards,” so that a harder material yields a higher number.

surfacepreload F₀Reset the instrumenttotal load F₀ + F₁the tip sinksreturn to F₀read the depth andreference (depth at F₀)and120° cone
Figure 19.11 · The principle of the Rockwell C test, with the indentation depths greatly magnified. The zero point is established after the preload; the hardness is determined from the permanent indentation, measured after removing the additional load.
Rockwell Hardness
HRC = 100 − e0.002 HRB = 130 − e0.002
and permanent indentation in mm, measured relative to the position after preload. Scale C: diamond cone with a 120° angle and rounded tip (radius 0.2 mm), total load 1471 N (150 kgf), for hardened and tempered steels, usable range 20–70 HRC. Scale B: 1.5875 mm (1/16 inch) ball, total load 980.7 N (100 kgf), for mild steels, brass, and light alloys, usable range 20–100 HRB.
Example 19.14 · From Depth to Rockwell Number

On a hardened high-speed steel end mill, the durometer measures a permanent indentation of 0.076 mm (scale C). On a mild steel round bar, using scale B, the indentation is 0.090 mm.

HRC = 100 − 0.076 / 0.002 = 100 − 38 = 62
HRB = 130 − 0.090 / 0.002 = 130 − 45 = 85
62 HRC for the tool, 85 HRB for mild steel

There are many other scales (A, D, E, F, G, H, K) and the surface scales N and T, which use smaller loads, for thin workpieces and treated layers: for example, HR15N or HR30N. In the workshop, however, one encounters almost exclusively HRC and HRB. Practical rules: the workpiece must be at least ten times as thick as the indentation depth, securely supported, and perpendicular to the indenter; on small round workpieces, the reading is slightly low and should be corrected using the tables in the standard; the first indentation after changing the workpiece or anvil is not counted.

Portable Hardness Testers

When a workpiece is too large to fit under a bench-top hardness tester (such as a ship’s shaft, a casting weighing several metric tons, or a mold mounted in a press), portable instruments are used. The most common is the Leeb rebound hardness tester: a small body with a carbide tip is launched against the surface, and the instrument measures its velocity before and after impact. The harder the material, the less energy it absorbs and the harder it rebounds. The Leeb number is HL = 1000 · vr / vi, where vi is the impact velocity and vr is the rebound velocity: with 2.05 m/s on the way out and 1.62 m/s on the way back, we have HL = 1000 · 1.62 / 2.05 = 790. The instrument then converts the value to HB, HV, or HRC using different tables for each material family, so you must select the correct material. There are also portable ultrasonic hardness testers (UCI method), which create a small Vickers indentation and are suitable for thin workpieces. These measurements are convenient but only indicative: for a binding test, one must use a bench-top hardness tester.

19.11 Conversions Between Hardness and Strength

The various tests measure different things (indentation area or depth, using different indenters and loads), so there is no exact formula for converting from one to another. However, there are experimental conversion tables derived from testing the same steels using all the methods (UNI EN ISO 18265). The table below was compiled by us using three approximate relationships, valid for unhardened carbon and low-alloy steels: they are useful for getting a general idea, but not for actual testing.

Approximate Equations for Steels (Rules of Thumb)
HB ≈ 0.95 · HV HRC ≈ 116 − 1500√HV Rm ≈ 3.4 · HB
HB Brinell hardness · HV Vickers hardness · HRC Rockwell C hardness (this is our own formula, valid only between 20 and 65 HRC, with errors of one or two points) · Rm tensile strength in N/mm², estimated only for steels and only up to approximately 1600 N/mm². These relationships do not apply to cast iron, light alloys, and work-hardened stainless steel.
HVHB (≈ 0.95 × HV)HRCRm ≈ 3.4 · HB (N/mm²)For example
120114-388S235 structural steel
150143-485S355, normalized C45
200190-646C45 (low values)
25023821808average reclamation
3002852996942CrMo4, heat-treated
350333361131high-strength reinforced
400380411292springs, heavily loaded shafts
450428451454hard reclaimed land
500475491615Upper bound of the estimate of Rm
55052352-molds, blades
60057055-hardened workpieces
65061857-Brinell hardness limit
700-59-bearings, calipers
800-63-high-speed steel tools

Approximate values, rounded, calculated using the three formulas above. The dash indicates that the scale is not used in that range (below 20 HRC, the scale switches to HRB or HB; above 650 HBW, the ball cannot withstand the pressure). For testing and disputes, the official tables in the standard are used.

The relationship Rm ≈ 3.4 · HB is the one most commonly used in the workshop: while it is not possible to cut a tensile test workpiece from a finished part, a hardness indentation is always made. This also aligns with the values in Section 10.4: an S235 with Rm = 400 N/mm² has approximately 400 / 3.4 = 118 HB, while a quenched and tempered 42CrMo4 with Rm = 1000 N/mm² has approximately 294 HB, which is around 31 HRC.

Example 19.15 · Estimating Strength Based on Hardness

The workpiece in Example 19.10 has a hardness of 206.6 HBW; the one in Example 19.12 has a hardness of 268.7 HV. Estimate Rm. Next: a drawing specifies 58 HRC; what is the corresponding value in HV?

First workpiece: Rm ≈ 3.4 × 206.6 = 702 N/mm² (the quenched and tempered C45 steel in the table in Section 10.4 has a value of 700 ✓)
Second workpiece: HB ≈ 0.95 × 268.7 = 255; Rm ≈ 3.4 × 255 = 868 N/mm²; HRC ≈ 116 − 1500 / √268.7 = 116 − 91.5 = 24.5
58 HRC: using the formula, HV ≈ (1500 / (116 − 58))² = (1500 / 58)² = 25.86² = 669
Rm ≈ 700 and ≈ 870 N/mm²; 58 HRC ≈ 670 HV: estimates to be used as a rough guide

19.12 Fatigue Testing

A workpiece that can withstand a static load very well may break if the load is applied and released millions of times, even with stresses well below the yield strength: this is fatigue failure, as discussed in Section 10.14. The most common fatigue test is the rotating bending test: a round, polished test specimen rotates under the load of a weight, so that with each rotation, every fiber on the surface alternates between tension and compression. A revolution counter records how many cycles the specimen withstands before breaking.

Many test specimens are tested, each at a different stress level, and the results are plotted on a stress-cycle-number graph, with cycles on a logarithmic scale: this is the Wöhler curve (Figure 10.11). For steels, the curve becomes horizontal after a few million cycles: the stress at which it flattens out is the fatigue limit σf; by convention, the test is stopped at 10 million cycles. For smooth steel test specimens, σf is approximately half of Rm. Light alloys do not have a true limit, and values are given at a fixed number of cycles. The test is lengthy (at 3,000 rpm, 10 million cycles take more than two days for a single specimen), and the results vary widely; therefore, analysis is based on averages and probabilities.

Rotational Bending Test on a Round Specimen
σ = MW = 32 · Mπ · d³ steel: σf ≈ 0,5 · Rm
σ maximum alternating stress on the surface in N/mm² · M bending moment in N·mm · W module of resistance in mm³ · d specimen diameter in mm · σf fatigue limit of the smooth specimen in N/mm² · Rm tensile strength in N/mm²
Example 19.16 · A Rotating Bending Specimen

An Ø8 mm test specimen made of quenched and tempered C45 steel (Rm ≈ 700 N/mm²) is rotated under a torque of 12 N·m. Will it break? What torque will cause it to reach the estimated fatigue limit?

σ = 32 × 12,000 / (π × 8³) = 384,000 / 1,608.5 = 238.7 N/mm²
Estimated limit: σf ≈ 0.5 × 700 = 350 N/mm² → 238.7 < 350; the test specimen should exceed 10 million cycles
Ultimate moment: M = σf · π · d³ / 32 = 350 · 1608.5 / 32 = 17,593 N·mm ≈ 17.6 N·m
At 12 N·m, the test specimen does not break; above approximately 17.6 N·m, it enters the limited-life zone

19.13 Non-Destructive Testing

The tests we’ve seen so far either break or mark the workpiece. To inspect a real workpiece—such as a casting, a weld, a forged shaft, or a workpiece returned from service—we need methods that can detect defects without damaging it: these are known as non-destructive testing (NDT). These tests are performed by qualified and certified operators (UNI EN ISO 9712), because the results depend heavily on the experience of the inspector. The first inspection is always a visual one, performed under good lighting using a magnifying glass and a mirror.

Penetrating fluids

They detect surface defects (cracks, porosity, folds) on any non-porous material, whether metallic or non-metallic. The workpiece is cleaned and degreased, then a very fluid colored (red) or fluorescent liquid is applied, which penetrates the cracks by capillary action; after a waiting period, the excess is removed from the surface, and a white developer—a very fine powder that absorbs the liquid remaining in the cracks—is sprayed on, causing drawings of the cracks to appear red (or yellow-green under an ultraviolet lamp). It is inexpensive and simple, but it cannot detect anything beneath the surface.

cleaningdegreased surfacepenetrating agentlet it sitRinseremains only in the crackdetectorthe crack “bleeds”
Figure 19.12 · Penetrant testing: cleaning, applying the penetrant, removing excess penetrant, and using a developer. The crack, invisible to the naked eye, appears as a large, clearly visible red stain.

Magnetic Imaging

It is used only on ferromagnetic materials (carbon and alloy steels, cast iron; not on aluminum, copper, or austenitic stainless steel). The workpiece is magnetized using a yoke or by passing an electric current through it, and a very fine iron powder—often suspended in a fluorescent liquid—is sprayed onto it. Where there is a crack, the magnetic field lines are forced to exit the workpiece, and the powder accumulates right there. It detects surface defects and those just below the surface (a few millimeters deep), provided they are oriented perpendicular to the magnetic field lines; for this reason, the workpiece is magnetized in two directions.

The particles cluster above the crackmagnetic field lines, shown in blue: in front of the crack, they exit the workpieceand attract the iron powder (or fluorescent liquid)NS
Figure 19.13 · Magnetic particle testing. A crack perpendicular to the magnetic field causes the magnetic lines of force to emerge: the magnetic particles accumulate and draw the defect.

Ultrasound

They detect internal defects and measure thicknesses. A probe placed against the workpiece, with a gel that displaces air, sends out very high-frequency sound pulses (from 1 to 10 MHz) that travel through the metal. When the sound waves encounter a surface—such as the bottom of the workpiece or a defect (a crack, a blowhole, or an inclusion)—part of the sound returns as an echo. The instrument measures the round-trip time and, knowing the speed of sound in the material, calculates the depth of the reflector. The screen displays the initial pulse, the background echo, and, if present, the echo from the defect in between.

probedefectbottom of the workpieces05101520pulsedefect echobackground echoround-trip time (µs)
Figure 19.14 · Ultrasonic inspection of a 60-mm-thick steel workpiece. On the screen, the echo from the defect arrives at 10.1 µs, and the echo from the bottom arrives at 20.3 µs (Example 19.17).
Reflector Depth
s = v · t2
s: depth of the defect (or thickness) in mm · v: speed of sound in the material in mm/µs (steel: approximately 5.92; aluminum: approximately 6.32 for longitudinal waves) · t: round-trip time in µs. This value is divided by 2 because the sound travels the distance twice.
Example 19.17 · At what depth is the defect?

In a steel block, the echo from a defect arrives after 10.1 µs. The speed of sound in steel is 5,920 m/s.

v = 5,920 m/s = 5.92 mm/µs
s = 5.92 × 10.1 / 2 = 29.9 mm
The defect is about 30 mm below the surface where the probe rests

X-ray

X-rays (or gamma rays from a radioactive source, for thick materials) pass through the workpiece, and on the other side, a film or digital detector records how much radiation passes through. Where there is a void (a blow, a porosity, or a lack of fusion in a weld), the material is thinner and the film appears darker. This produces an image that serves as a record, and it is the standard method for welds and castings; however, it requires protected areas and authorized personnel, and it does not detect fine cracks parallel to the beam very well. Industrial computed tomography takes multiple X-ray images from different angles and reconstructs the workpiece in three dimensions, including for measurement purposes (Chapter 37).

Induced currents

A coil through which an alternating current flows, when brought close to a conductive workpiece, induces circular currents in the metal, the induced currents (or interference). A superficial crack disrupts it, and the coil detects this because its impedance changes. The method is fast, non-contact, and easily automated: it is used to inspect tubes and bars on the production line, check rivet holes in aircraft, measure the thickness of paints and coatings, and sort workpieces or treatment stages that have been mixed up by error.

MethodWhat flaws does he find?What materialsMain Limitations
Visualmajor defects, shapes, finishingeveryoneHe sees only what is visible
Penetrating fluidscracks and open pores on the surfaceall non-porous materialsNothing beneath the surface; thorough cleaning
Magnetic Imagingon the surface and just below the surfaceonly ferromagnetic materialsdefects across the field; demagnetize afterward
Ultrasoundinternal dimensions, including depth; thicknessesalmost all metalsexperienced operator; complex shapes; coarse-grained cast iron
X-rayinternal voids, porosity, inclusionseveryoneradiation protection; thin, misaligned cracks
Induced currentssuperficial cracks; coating thicknessesonly conductorsinsufficient depth; a reference sample is needed

19.14 Technological Tests and Material Selection

Technological tests do not measure a physical quantity: they verify whether the material can withstand certain machining operations or use by simulating them on a small scale. The result is often a “pass” or “fail.”

Bending Test

A bar or strip of sheet metal with thickness a is bent around a spindle with diameter D to a specified angle (often 180°). The outer grain—the most elongated one—is then examined: if there are no visible cracks, the test is passed. The spindle diameter is specified by the product standard or specifications, as a multiple of the thickness (for example, D = 2 · a or 3 · a): the smaller the spindle, the more rigorous the test. This test is performed on sheet metal, reinforcing bars, and especially on welded joints to detect casting defects in the weld bead.

Fspindlebefore the testDtoouter fiber:the most elongatedAfter a 180° bendcheck the outer fiber for cracks
Figure 19.15 · Bending test: The test specimen, with thickness a, is bent around a spindle with diameter D. Here, D = 3 · a, as in Example 19.18.
Elongation of the outer fiber at the fold
εeast = aD + a · 100 (%)
ε is the elongation of the outer fiber in % · a is the thickness of the test specimen in mm · D is the diameter of the spindle in mm. It is calculated by comparing the outer fiber (radius D/2 + a) with the middle fiber, which does not elongate (radius (D + a)/2).
Example 19.18 · How much does the outer fiber stretch?

A 10-mm-thick plate is bent 180° on a Ø30 spindle (D = 3 · a).

Radius of the inner fiber: (30 + 10) / 2 = 20 mm; radius of the outer fiber: 15 + 10 = 25 mm
εest = (25 − 20) / 20 × 100 = 10 / (30 + 10) × 100 = 25%
The outer fiber stretches by 25%: a steel with A around 26% passes the test, while a quenched and tempered steel with A = 14% is at risk of cracking

Erichsen Deep Drawing and Other Tests

The Erichsen test is used for sheet metal intended for deep drawing: a punch with a spherical head pushes the sheet metal, which is clamped all around, until a dome forms and the first crack appears. The depth reached, in millimeters, is the Erichsen index: the higher it is, the more suitable the sheet metal is for deep drawing (Chapter 23). Other, more specialized technological tests include the flattening and flaring of tubes, cold heading of fastener bars, and torsion testing of wires.

Choose the material by looking at the samples

Each workpiece request requires you to look up a specific number. The table serves as a reference when reading a certificate or selecting steel from inventory.

The workpiece must...You lookTest
support the load without deforming, indefinitelyRe o Rp0,2traction
does not break, even when overloadedRm, Re/Rm ratiotraction
bends very little (stiffness)Module E (and the shape of the workpiece)tensile test with an extensometer
to be bent, stamped, or rivetedA%, Z%, Erichsen indextensile testing, bending, Erichsen
be impact- and cold-resistantKV at the minimum operating temperatureCharpy
Don't wear yourself out; stay focused.HRC or HVhardness
spin or vibrate for yearsfatigue limit, finishingeffort
to be weldedcarbon equivalent (CE)chemical analysis, joint bending
be free of internal defects (castings, welds, forgings)results of the inspectionultrasound, X-ray

The test results arrive at the shop on certificate from the supplier. According to the UNI EN 10204 standard, the type 2.2 It is a statement containing non-specific test results (conducted on the production run in general); the type 3.1 It includes the test results for that specific batch, signed by a representative of the manufacturer who is independent of the production process. For critical workpieces, a 3.1 report is required and must be retained along with the casting number, which must also be marked on the material.

Example 19.19 · Verifying a Certificate 3.1

A 20-mm-thick S355J2 steel plate has arrived. The certificate states: ReH = 378 N/mm², Rm = 541 N/mm², A = 27%, KV at −20 °C for the three test specimens: 64, 71, and 58 J. For that thickness, the standard requires (approximate values; verify against the current standard): ReH ≥ 345 N/mm², Rm between 470 and 630 N/mm², A ≥ 22%, average KV ≥ 27 J at −20 °C.

Yield strength: 378 ≥ 345 ✓ ; Tensile strength: 470 ≤ 541 ≤ 630 ✓ ; Elongation: 27 ≥ 22 ✓
Average resilience: (64 + 71 + 58) / 3 = 193 / 3 = 64.3 J ≥ 27 ✓ (and no single value is too low)
yield ratio: 378 / 541 = 0.70
The material complies with specifications: it is accepted, and the pour number is recorded

7:15 p.m. The formulas in this chapter

WhatFormula
Carbon equivalentCE = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
Proportional test tubeL0 = 5.65 · √S0 (round: L0 ≈ 5 · d0)
Stress and Strainσ = F / S0 · ε = ΔL / L0
ResistanceReH = FeH / S0 · ReL = FeL / S0 · Rp0.2 = Fp0.2 / S0 · Rm = Fm / S0
Elongation and ContractionA% = (Lu − L0) / L0 · 100 · Z% = (S0 − Su) / S0 · 100
Modulus of elasticityE = Δσ / Δε
Compression and Bendingσc = F / S0 · σf = 8 · F · L / (π · d³)
CharpyKV = m · g · (h1 − h2) = m · g · R · (cos β − cos α)
BrinellHBW = 0.102 · 2F / (π · D · (D − √(D² − d²))) · F = 9.807 · k · D²
VickersHV = 0.1891 · F / d² · d = (d1 + d2) / 2
RockwellHRC = 100 − e / 0.002 · HRB = 130 − e / 0.002
LeebHL = 1000 · vr / vi
Approximate conversions (steels)HB ≈ 0.95 · HV · HRC ≈ 116–1,500 / √HV · Rm ≈ 3.4 · HB
Rotational Bending Fatigueσ = 32 · M / (π · d³) · σf ≈ 0,5 · Rm
Ultrasounds = v · t / 2
Foldingεest = a / (D + a) · 100

19.16 Exercises

Use g = 9.81 m/s² and the data from the table in Section 10.4 when they are not given in the text. Try to solve the problems on your own first, then check the solution.

Exercise 1. What should be the length between the reference points of a short proportional test tube with a diameter of 12 mm?
Solution

S0 = π · 12² / 4 = 113.10 mm²; L0 = 5.65 · √113.10 = 5.65 · 10.635 = 60.09 mm, or 60 mm.

Exercise 2. A test specimen with a diameter of 10 (L0 = 50 mm) has FeL = 27.9 kN, Fm = 40.1 kN, and Lu = 61.0 mm after fracture. Calculate ReL, Rm, and A%. What type of steel could this be?
Solution

S0 = 78.54 mm²; ReL = 27,900 / 78.54 = 355.2 N/mm²; Rm = 40,100 / 78.54 = 510.6 N/mm²; A = (61 − 50) / 50 × 100 = 22%. It is S355.

Exercise 3. In the same test tube, the minimum diameter after fracture is 6.4 mm. What is the value of the constriction?
Solution

Su = π · 6.4² / 4 = 32.17 mm²; Z = (78.54 − 32.17) / 78.54 · 100 = 59.0%.

Exercise 4. A Ø10 test specimen made of an aluminum alloy, with a strain gauge set at L0 = 50 mm, stretches by 0.0455 mm under a load of 5 kN, still within the elastic range. Calculate the module of elasticity.
Solution

σ = 5,000 / 78.54 = 63.66 N/mm²; ε = 0.0455 / 50 = 0.000910; E = 63.66 / 0.000910 = 69,958 N/mm², approximately 70,000 N/mm² (typical for aluminum alloys).

Exercise 5. Brinell test using a 10-mm ball and 29,420 N: the indentation measures 3.60 mm. Calculate the hardness and estimate Rm.
Solution

3.60 / 10 = 0.36 (valid). √(100 − 12.96) = 9.3295; D − 9.3295 = 0.6705 mm; HBW = 0.102 · 2 · 29,420 / (π · 10 · 0.6705) = 6,001.7 / 21.064 = 284.9, i.e., 285 HBW 10/3000. Rm ≈ 3.4 · 284.9 = 969 N/mm²: a quenched and tempered 42CrMo4 steel.

Exercise 6. HV10 test (F = 98.07 N): The diagonals measure 0.281 and 0.287 mm. What is the hardness value?
Solution

d = (0.281 + 0.287) / 2 = 0.284 mm; d² = 0.080656 mm²; HV = 0.1891 · 98.07 / 0.080656 = 229.9, or 230 HV10.

Exercise 7. In a Rockwell C test, the permanent indentation is 0.094 mm. What is the hardness value? And what indentation does a mild steel with a hardness of 80 HRB produce?
Solution

HRC = 100 − 0.094 / 0.002 = 100 − 47 = 53 HRC. For 80 HRB: e = (130 − 80) · 0.002 = 0.100 mm.

Exercise 8. The pendulum bob of a Charpy pendulum has a mass of 18 kg and starts at a height of 1.60 m. After breaking a test specimen tested at −40 °C, it returns to a height of 1.32 m. Calculate KV. Is the steel suitable for that temperature if at least 27 J is required?
Solution

KV = 18 · 9.81 · (1.60 − 1.32) = 176.58 · 0.28 = 49.4 J (initial energy 282.5 J, residual energy 233.1 J). 49.4 ≥ 27: yes.

Exercise 9. A pendulum with a 20-kg bob at a distance of 0.80 m from the pivot has an initial angle of 150°. After breaking, it returns to 110°. What is the value of KV?
Solution

cos 110° = −0.3420; cos 150° = −0.8660. KV = 20 × 9.81 × 0.80 × (−0.3420 + 0.8660) = 156.96 × 0.5240 = 82.2 J.

Exercise 10. A steel shaft has a hardness of 250 HB. Estimate the values of HV, HRC, and Rm using the relationships in Section 19.11.
Solution

HV ≈ 250 / 0.95 = 263.2; HRC ≈ 116 − 1500 / √263.2 = 116 − 92.5 = 23.5; Rm ≈ 3.4 × 250 = 850 N/mm². These are estimates.

Exercise 11. In a 60-mm-thick steel block, the background echo arrives at 20.0 µs and the echo from a defect arrives at 7.2 µs. Determine the speed of sound and the depth of the defect.
Solution

v = 2 · s / t = 2 · 60 / 20 = 6.0 mm/µs; defect depth s = 6.0 · 7.2 / 2 = 21.6 mm. (You can also use a proportion: 60 × 7.2 / 20 = 21.6 mm.)

Problem 12. A cast-iron bar with a diameter of 20 mm, supported at points 200 mm apart, breaks in the middle under a load of 6.6 kN. Calculate the bending strength.
Solution

M = 6,600 · 200 / 4 = 330,000 N·mm; W = π · 20³ / 32 = 785.4 mm³; σf = 330,000 / 785.4 = 420.2 N/mm².

Exercise 13. What force is required for a Brinell test on brass using a 2.5-mm ball and a load grade of 10? What indentation diameters are acceptable?
Solution

F = 9.807 × 10 × 2.5² = 612.9 N (62.5 kgf). The footprint must be between 0.24 × 2.5 = 0.60 mm and 0.6 × 2.5 = 1.50 mm.

Exercise 14. A steel contains 0.20% C, 1.20% Mn, 0.30% Cr, 0.20% Ni, and 0.30% Cu. Calculate the carbon equivalent: Can it be welded without preheating?
Solution

CE = 0.20 + 1.20 / 6 + 0.30 / 5 + (0.20 + 0.30) / 15 = 0.20 + 0.20 + 0.06 + 0.033 = 0.493. It’s above 0.45: it’s best to preheat and follow a procedure.