Chapter 20

Steels and Cast Irons

Almost everything that passes through a lathe or a milling machine is steel or cast iron. They are alloys of iron and carbon, but changing the carbon content by just a few tenths of a percent—or adding a little chromium, nickel, or molybdenum—is enough to transform a sheet of metal that can be bent by hand into a tool capable of cutting other steel. In this chapter, we’ll look at how they’re made, what they’re called (abbreviations like 42CrMo4 or X5CrNi18-10 will become easy to understand), what families exist, in what forms they’re sold, and how they behave under the tool.

20.1 From Ore to Steel

Iron does not occur in its pure form in nature: it is bound to oxygen in iron ores, especially hematite (Fe2O3) and magnetite (Fe3O4). Today, there are two methods used to produce steel: the full cycle that starts with the ore and the scrap cycle which starts with scrap steel.

The blast furnace

A blast furnace is a tower that can be over 30 meters tall. From the top, ore, coke (baked coal, which serves as both fuel and a reducing agent), and limestone (which absorbs impurities) are loaded in layers. Hot air is blown in from the bottom. The coke burns, producing carbon monoxide that strips oxygen from the ore, and the iron melts as it sinks toward the bottom. Along the way, however, it absorbs a great deal of carbon: what emerges, at around 1450–1500 °C, is blast furnace cast iron containing about 4–4.5% carbon, plus silicon, manganese, phosphorus, and sulfur. Floating on top of the cast iron is the slag, which is used in cement production.

The oxygen converter

Blast furnace cast iron contains too much carbon to be processed: it is hard and brittle. It is therefore poured, while still liquid, into a converter—a large, pear-shaped vessel—along with some scrap metal. A water-cooled lance blows pure oxygen onto the molten metal: the carbon burns and escapes as a gas, while the other impurities pass into slag. In about twenty minutes, the cast iron becomes steel. It is this reaction that generates heat—so much so that the added scrap metal also serves to prevent the temperature from rising too high.

The Electric Arc Furnace

The second method starts with scrap: scrapped cars, offcuts from machining operations, and compressed chips. It is loaded into a furnace with three large graphite electrodes; electric arcs jump between the electrodes and the scrap, melting it. This is the most common method in Italy, where most steel is produced this way: steel can be recycled an infinite number of times without losing quality, and it is the most recycled material in the world.

Refining and Continuous Casting

The molten steel passes into a ladle—a large container lined with refractory material—where refining (secondary metallurgy) takes place: ferroalloys are added to achieve the correct composition, dissolved oxygen is removed (deoxidation), and, for higher-purity steels, gases are removed under vacuum. Then comes continuous casting: the steel flows from a trough (the ladle) into a water-cooled copper mold, where a solid skin forms; the bar, still liquid inside, is pulled through a series of rollers, bent, straightened, and cut to size with a cutting torch. This produces the semi-finished products: billets (small square cross-section), blooms (large square cross-section), and slabs (wide, flat rectangular cross-section). From here, through hot rolling and then, if necessary, cold rolling, bars, wire rod, shapes, and sheet metal are produced (Chapter 23).

ore, coke, limestoneblast furnacemolten cast ironapproximately 4.5% Coxygenoxygen convertersteel scrapgraphite electrodeselectric arc furnaceladlerefiningladleingot moldcooledrollerscuttingbillets, blooms, slabsthen rolling: bars, sheet metal, structural steel
Figure 20.1 · The two steelmaking processes: ore, blast furnace, and converter (top), or scrap and electric furnace (bottom). Both end up in a ladle and then in the continuous casting process.
Example 20.1 · How much carbon does the converter burn?

100 metric tons of cast iron containing 4.5% carbon are fed into the converter. The goal is to produce steel containing 0.2% carbon. How much carbon must be burned, assuming that only carbon is lost?

Initial carbon: 100 · 4.5 / 100 = 4.5 t
If x is the number of metric tons of carbon burned, the steel weighs 100 − x and contains 0.2% carbon: 4.5 − x = 0.002 · (100 − x)
4,5 − x = 0,2 − 0,002x → 4,3 = 0,998x → x = 4,309 t
Steel produced: 100 − 4.309 = 95.69 metric tons, containing 0.191 metric tons of carbon
About 4.3 metric tons of carbon are burned: almost all of what was there

20.2 Iron, Steel, and Cast Iron: The Role of Carbon

Pure iron is soft, ductile, and not very strong: on its own, it is of little use in mechanical engineering. Adding carbon changes everything, because carbon settles between the iron atoms and forms an extremely hard compound with them, called cementite (Fe3C). It is carbon itself that draws the line between steel and cast iron:

  • steel: an alloy of iron and carbon less than 2% approximately (the theoretical value is 2.06%; some sources list 2.11%). It can be rolled, forged, bent, and, if there is enough carbon, hardened;
  • cast iron: carbon content above 2%, typically between 2.5 and 4%. It cannot be forged or rolled, but it melts at a lower temperature and fills molds well: it is the material used for castings (workpieces cast in a mold).
STEELSCAST IRON01234% C2.06%4.3%Enlarged section belowcast iron: 2.5–4% Cferrite + perliteperlite + cementite0.00.20.40.60.81.01.2% CC15C45C600.77%100Cr6structural steels: almost all between 0.1 and 0.6% C
Figure 20.2 · Above: the entire range from 0 to 4.5% carbon. Below: a magnified view of the range of steels most commonly machined on machine tools.

Ferrite, perlite, and cementite

When viewed under a microscope after slow cooling, carbon steel exhibits two phases. Ferrite is nearly pure iron (it dissolves very little carbon—at most 0.02%): it is soft and ductile. Pearlite is an interlaced network of extremely thin lamellae of ferrite and cementite: it is harder and more durable. At 0.77% carbon (eutectoid steel), the structure consists entirely of pearlite; below this temperature, the structure consists of ferrite and pearlite, and above this temperature, of pearlite and cementite. For this reason, up to about 0.8%, adding carbon increases hardness and strength while reducing elongation. We’ll see what happens when steel is heated and cooled rapidly (hardening) in Chapter 22.

Perlite in slowly cooled carbon steel (estimate)
perlite % ≈ C0,77 · 100 (for C ≤ 0.77%)
C is the carbon content of the steel in % · 0.77 is the carbon content of the perlite in %. The formula neglects the 0.02% dissolved in the ferrite; it yields a value slightly higher than the exact one.
C15approximately 19% perliteC45approximately 58% perlite0.77% C100% perlite
Figure 20.3 · Schematic diagram of grains (not a photograph): ferrite grains are white, and pearlite grains are striped. The more carbon, the more pearlite.
Example 20.2 · How much perlite is there in a C15 and a C45?
C15 (0.15% C): perlite ≈ 0.15 / 0.77 × 100 = 19.5%
C45 (0.45% C): perlite ≈ 0.45 / 0.77 × 100 = 58.4%
using the exact formula, which accounts for the 0.02% in the ferrite: C45 → (0.45 − 0.02) / (0.77 − 0.02) · 100 = 57.3%
C15 is almost entirely ferrite (malleable, welds well); C45 is more than half pearlite (stronger, can be hardened)

20.3 Alloying Elements

In addition to carbon, every steel contains other elements. Some are always present because they result from the manufacturing process (manganese and silicon, used for deoxidation); others are impurities that must be kept to a minimum (sulfur and phosphorus); and still others are added intentionally to impart specific properties: these are the alloying elements. Based on the number of alloying elements present, the EN 10020 standard classifies steels as unalloyed (no element exceeding the standard’s thresholds, for example, manganese below 1.65%) and alloyed; in the designation (paragraph 20.5), a distinction is then made between low-alloy steels, with each element below 5%, and high-alloy steels, with at least one element at 5% or more.

ElementWhat does it do to steel?Where is it located?
Carbon CIncreases hardness, strength, and hardenability; reduces elongation, weldability, and—at levels above 0.5%—machinabilityin all of them; from 0.05% to over 1.5%
Mn manganeseIt reduces oxygen, binds with sulfur (manganese sulfide), and renders it harmless; it increases strength and hardenabilityin all (0.3–1.5%); 16MnCr5, 28Mn6
Yes, silicondeoxidizer; increases yield strength and elasticity; improves the magnetic properties of the laminationsspring steel (54SiCr6), motor laminations
Cr chromiumIncreases hardenability and wear resistance (forms hard carbides); at levels above 10.5%, it makes the steel stainless42CrMo4, 100Cr6, stainless steel, tool steels
No nickelIt increases toughness, even at low temperatures, and hardenability; in stainless steels, it produces an austenitic structure39NiCrMo3, 34CrNiMo6, austenitic stainless steels
Mo (molybdenum)Increases hardenability, reduces brittleness after tempering, and improves heat resistance; in stainless steel, it protects against pitting corrosion42CrMo4, AISI 316 stainless steel, high-speed steels
Vanadium Vrefines the grain, forms extremely hard carbides (wear resistance), maintains hardness at high temperatures51CrV4, tool steels and high-speed steels
Tungsten (W)forms extremely hard carbides; retains its hardness at high temperatureshigh-speed steels, steels for hot machining operations
S (sulfur)an impurity that makes the material brittle when hot; desired in automatic machines because sulfides break up the chipslimited to approximately 0.035%; 0.2–0.4% in automatic machines
P phosphorusan impurity that makes it brittle when cold and when subjected to impactlimited to 0.025–0.045%
Pb leadIt does not melt: it remains in droplets that lubricate the cutting edge and break up the chips; it reduces fatigue strength and weldabilityautomatic (11SMnPb37), 0.15–0.35%

Table prepared by CNC Simulator Italia: main effects, simplified. Other useful elements: aluminum (deoxidizes, refines the grain, forms nitrides in nitriding steels), cobalt (hot hardness in high-speed steels), boron (just a few thousandths of a percent is enough to increase hardenability), titanium and niobium (bind carbon in stainless steels).

💡
Hardenability does not mean hardness. The maximum hardness after hardening depends almost entirely on carbon. Alloying elements serve to harden the workpiece to a greater depth and with less severe cooling (in oil rather than water, resulting in less distortion and cracking). Surface-hardened C45 and 42CrMo4 achieve similar hardness levels; on an 80-diameter shaft, however, the core of the 42CrMo4 remains much more durable.

20.4 Designation for Use (EN 10027-1)

The EN 10027-1 standard assigns symbolic designations to steels that serve as a sort of identification card. There are two main groups of designations: those that indicate the steel’s intended use and its strength (Group 1, for application) and those that indicate its composition (Group 2, for chemical composition, paragraph 20.5).

In designations for specific applications, the first letter indicates the intended use, and the number immediately following it usually indicates the minimum yield strength Re in N/mm² for the thinnest gauges (Chapter 10). This is followed, if necessary, by letters and numbers indicating other properties.

LetterEmploymentExamples
Ssteel for structural applications (structural steelwork, frames, brackets)S235JR, S275J0, S355J2
Esteels for mechanical engineering (shafts, pins, levers—untreated)E295, E335, E360
Psteels for pressure vesselsP265GH
Lsteel for pipeline pipesL360
Bsteel for reinforced concreteB450C
DCCold-rolled sheets for cold forming (the number indicates quality, not yield strength)DC01, DC04

For S steels, the designation continues with the resilience value—that is, the energy the material absorbs when it fractures during an impact test (Chapter 19): the lower the temperature at which resilience is guaranteed, the better the steel resists impact at low temperatures.

SymbolMinimum energyTest temperature
JR27 J+20 °C
J027 J0 °C
J227 J−20 °C
K240 J−20 °C

At the end of the designation, following a + sign, you can indicate the supply condition or heat treatment: +N normalized, +A annealed, +QT quenched and tempered, +C cold-worked (e.g., drawn). The heat treatments are explained in Chapter 22.

S355J2+NSstructural use355Minimum yield strength 355 N/mm²Thicknesses up to 16 mmJ227 J at −20 °CImpact test+NSuppliednormalized
Figure 20.4 · How to read an application code: S355J2+N.
Example 20.3 · Read three abbreviations for job titles
S235JR → structural steel, Re ≥ 235 N/mm², impact strength 27 J at +20 °C: the most common structural steel
S355J2+N → structural, Re ≥ 355 N/mm², 27 J at −20 °C, normalized: for welded structures subject to higher loads or operating in cold conditions
E295 → structural steel for mechanical engineering, Re ≥ 295 N/mm²; the standard does not specify the chemical composition, so it is not suitable for heat treatment or heavy-duty welding
The letter specifies the intended use, the minimum number required, and the rest are additional guarantees.
📏
The yield strength decreases with thickness. The number in the designation applies to thinner products. A 50-mm-thick S355 has a guaranteed minimum yield strength lower than 355 N/mm², because workpieces cool more slowly in the steel mill. For calculations, use the standard value for the actual thickness.

20.5 Designation by Chemical Composition

For structural, heat-treated, stainless, and tool steels, the composition is what matters, and the designation reflects it. There are four cases.

Unalloyed Steels

The letter C followed by the average carbon content multiplied by 100. C45 refers to non-alloy steel with approximately 0.45% carbon (within the standard range of 0.42–0.50%). A letter at the end provides information on sulfur: C45E has the maximum prescribed sulfur content (low, for better toughness), while C45R has sulfur within a range (slightly higher, for better machinability).

Example 20.4 · Unalloyed Steels
C15 → 15 / 100 = 0.15% C: mild steel, case-hardening steel, or steel for welded workpieces
C45 → 45 / 100 = 0.45% C: the classic unalloyed quenched-and-tempered steel
C60 → 60 / 100 = 0.60% C: harder, for workpieces subject to wear and for simple springs
In non-metallic compounds, the abbreviation primarily refers to carbon

Low-alloy steels

No single item reaches 5%. The formula is as follows:

  • a number = average carbon × 100 (without the letter C in front);
  • the chemical symbols of the alloying elements in descending order of content;
  • numbers indicating the content of the elements, in the same order as the symbols, each multiplied by a factor; if there is more than one number, they are separated by a hyphen. The elements following the last number do not have a specified content: the notation simply indicates that they are present.
From the grade number to the percentage (low-alloy steels)
C % = initial number100 element % = element numberfactor
Factors: 4 for Cr, Co, Mn, Ni, Si, W · 10 for Al, Be, Cu, Mo, Nb, Pb, Ta, Ti, V, Zr · 100 for Ce, N, P, S · 1,000 for B. The factor is larger for elements used in smaller quantities: thus, the symbol number is always an integer. The result is an indicative average value: the actual limits are specified in the material standard.
42CrMo442 / 1000.42% carbonCr and Moin descending order of contentdecreasing4 / 4 = 1% CrMo not listed:present, in small amounts X5CrNi18-10Xhigh-alloy(one element ≥ 5%)5 / 1000.05% carbonCr and Nialloying elements18% Cr, 10% Niactual percentages,without a factor HS6-5-2-5HShigh-speed(high-speed)W 6 · Mo 5 · V 2 · Co 5percentages, alwaysin this order
Figure 20.5 · Three designations for chemical composition: a low-alloy steel (42CrMo4), a high-alloy steel (X5CrNi18-10), and a high-speed steel (HS6-5-2-5).
Example 20.5 · The Composition of 42CrMo4
42 → carbon 42 / 100 = 0.42%
Elements: Cr and Mo; chromium is the more abundant of the two
a single number, 4, which corresponds to the first element: Cr = 4 / 4 = 1%
Mo is not listed: it is present, but in small quantities (typically 0.15–0.30%)
Comparison with the standard: C 0.38–0.45% and Cr 0.90–1.20%—the measured values fall within this range
42CrMo4 ≈ 0.42% C, 1% Cr, a small amount of Mo: chromium-molybdenum quench-and-temper steel
Example 20.6 · The Percentage Composition of 39NiCrMo3
39 → carbon 39 / 100 = 0.39%
Elements in descending order: Ni, Cr, Mo
a single number, 3, for nickel (factor 4): Ni = 3 / 4 = 0.75%
Unspecified amounts of Cr and Mo (typically about 0.6–1.0% Cr and 0.15–0.25% Mo)
39NiCrMo3 ≈ 0.39% C, 0.75% Ni, plus Cr and Mo: a tough quenched-and-tempered steel, widely used in Italy
Example 20.7 · From Composition to Notation (Bass Slurs)

A nitriding steel contains, on average, 0.41% C, 1.75% Cr, 1.0% Al, and 0.25% Mo. A case-hardened steel for gears contains 0.18% C, 1.65% Cr, 1.55% Ni, and 0.30% Mo. Write the symbols, indicating the content of the first two elements.

First: carbon 0.41 × 100 = 41; in descending order: Cr, Al, Mo
Cr: 1.75 × 4 = 7; Al: 1.0 × 10 = 10 → 41CrAlMo7-10
second: carbon 0.18 × 100 = 18; order: Cr, Ni, Mo
Cr: 1.65 × 4 = 6.6 → 7; Ni: 1.55 × 4 = 6.2 → 6 → 18CrNiMo7-6
41CrAlMo7-10 and 18CrNiMo7-6 (the numbers are rounded to the nearest whole number)

High-alloy steels

At least one element makes up 5% or more. The notation begins with the letter X, followed by carbon × 100, then the symbols of the elements in descending order, and finally their actual percentages, rounded to whole numbers and separated by hyphens: there are no factors here.

High-speed steels

The letters HS (short for high speed) followed by the percentages of four elements, always in the same order: tungsten, molybdenum, vanadium, and cobalt. If cobalt is not present, there are three numbers.

Example 20.8 · Long ties and runs
X5CrNi18-10 → X: high-alloy; 5 / 100 = 0.05% C; 18% Cr; 10% Ni (this is AISI 304 stainless steel)
Composition: 0.02% C, 17% Cr, 12% Ni, 2.2% Mo → X2CrNiMo17-12-2 (this is AISI 316L stainless steel)
HS6-5-2-5 → high-speed steel with 6% W, 5% Mo, 2% V, 5% Co; a total of 6 + 5 + 2 + 5 = 18% of major elements, plus about 4% chromium and 0.9% carbon, which the designation does not specify
HS2-9-1-8 → 2% W, 9% Mo, 1% V, 8% Co: cobalt-based, molybdenum-rich
X and HS are changing the rule: the numbers are already percentages
✅
A quick check. If a number appears in a designation without an “X” that, when divided by its factor, yields more than 5%, there is an error: either it is a high-alloy steel and the “X” is missing, or the factor is incorrect. Reading 42CrMo4 without the factor would yield 4% chromium, which is not correct.
Example 20.9 · Ten Acronyms to Decode
AcronymTypeWhat does it say?
S275J0by usestructural, Re ≥ 275 N/mm², 27 J at 0 °C
E335by usemechanical engineering, Re ≥ 335 N/mm²
C22Eunbound0.22% C, maximum sulfur content specified
16MnCr5low note0.16% C; Mn = 5 / 4 = 1.25%; Cr present
34CrNiMo6+QTlow note0.34% C; Cr = 6 / 4 = 1.5%; Ni and Mo present; supplied heat-treated
51CrV4low note0.51% C; Cr = 4 / 4 = 1%; V present (spring steel)
11SMnPb37low note0.11% C; S = 37 / 100 = 0.37%; Mn and Pb present (automatic)
100Cr6low note1.00% C; Cr = 6 / 4 = 1.5% (bearings)
X153CrMoV12high legato1.53% C; 12% Cr; contains Mo and V (tools for cold machining operations)
HS6-5-2quick6% W, 5% Mo, 2% V, no cobalt
With three rules (factors, X, HS), you can decipher almost all workshop codes

20.6 Steel Designations (EN 10027-2)

In addition to its symbolic name, each type of steel has a material number, which is useful for inventory management systems and data sheets: it is often stamped on the bars or written on the certificates. The format is 1.GGNN:

  • 1 refers to the material group: 1 means steel (cast irons have their own numbering system; see paragraph 20.13);
  • GG, a two-digit number, is the steel group, according to the family;
  • NN, a two-digit number, is the sequence number within the group; it has no technical significance.
GG GroupFamilyExamples
00 e 90base steels1.0037 (former part number for the S235JR)
01-07 e 91-97non-alloy quality steels1.0503 C45 · 1.0715 11SMn30 · 1.0737 11SMnPb37
10-18non-alloy special steels1.1191 C45E · 1.1141 C15E
20-29alloy tool steels1.2379 X153CrMoV12 · 1.2344 X40CrMoV5-1
32-33high-speed steels (32 with cobalt, 33 without)1.3243 HS6-5-2-5 · 1.3343 HS6-5-2
35bearing steels1.3505 100Cr6
40-45stainless steels1.4301 X5CrNi18-10 · 1.4404 X2CrNiMo17-12-2
50-89alloy steels for construction and mechanical engineering1.7131 16MnCr5 · 1.7225 42CrMo4 · 1.6582 34CrNiMo6

Simplified list of the main groups. The grades of stainless steel, for example, also distinguish between nickel content below or above 2.5% and the presence of molybdenum: 1.43xx grades are stainless steels with at least 2.5% nickel and no molybdenum, while 1.44xx grades contain molybdenum.

1.72251steel72Group: Alloy Steelschromium-molybdenum25Order numberin the group
Figure 20.6 · The number 1.7225 refers to 42CrMo4: Group 72 includes chromium-molybdenum steels.
Example 20.10 · Four material numbers
1.0037 → base steel (group 00): this is the number used to designate S235JR (formerly German St 37-2); In the current standard, S235JR is designated as 1.0038, but the old designation is still found on drawings and in inventory
1.1191 → special non-alloy steel (Group 11): C45E, C45 with controlled sulfur content, suitable for heat treatment
1.7225 → alloy structural steel (Group 72, chromium-molybdenum): 42CrMo4
1.4301 → stainless steel (Group 43, at least 2.5% nickel and no molybdenum): X5CrNi18-10, i.e., AISI 304
The first digit after the decimal point is enough to identify the family: 0 and 1 are unalloyed; 2 and 3 are for tools, bearings, and high-speed applications; 4 is stainless steel; and 5 through 8 are alloyed structural steels.

20.7 Correspondences with AISI/SAE designations and with the old UNI standards

In the workshop, we sometimes receive American drawings (AISI/SAE designations—four digits for carbon and alloy steels, three digits for stainless steels) or older Italian drawings with UNI designations predating European standards (for example, Fe 360 or Fe 510 for structural steels). In four-digit SAE designations, the last two digits indicate the carbon content in hundredths of a percent: 1045 has about 0.45% C, like C45; the first two digits indicate the family (10 for unalloyed, 41 for chromium-molybdenum, 43 for nickel-chromium-molybdenum, 52 for chromium).

EN (name)NumberAISI/SAE equivalentSimilar to the old UNI
S235JR1.0038A36 (ASTM, for reference only)Fe 360 B
S355J21.0577A572 Grade 50 (ASTM, for reference only)Fe 510 D
C451.05031045C45
42CrMo41.7225414042CrMo4
34CrNiMo61.6582434035NiCrMo6
16MnCr51.7131511516MnCr5
100Cr61.350552100100Cr6
11SMnPb371.073712L14CF9SMnPb36
X5CrNi18-101.4301304X5CrNi1810
X2CrNiMo17-12-21.4404316LX2CrNiMo1712
X20Cr131.4021420X20Cr13
HS6-5-21.3343M2HS6-5-2

Approximate equivalencies, prepared by CNC Simulator Italia: the specifications of the various standards overlap only partially, and the guaranteed minimum values may differ. For a critical workpiece, compare the technical data sheets of the two standards or request a certificate from the supplier.

20.8 Families of structural steels for mechanical engineering

The designation indicates what's inside; the family indicates how it's used. Here are the families that a turner or miller encounters most often. Hardness values (HB, HRC) are explained in Chapter 19, and heat treatments in Chapter 22.

Structural Steels

S steels (S235, S275, S355) are used in structural steelwork: they weld well because they have a low carbon content, and they bend and cut easily. They are not hardened. E-grade steels (E295, E335) are used for lightly loaded mechanical parts that do not require heat treatment: pins, levers, and tie rods.

Quench-and-temper steels

They contain 0.25 to 0.6% carbon and are used in a heat-treated state—hardened and then tempered—to achieve both strength and toughness. These steels are used for shafts, axes, connecting rods, non-case-hardened gears, and high-strength screws. C45 is the most economical but hardens well only in thin sections; alloy steels such as 42CrMo4, 39NiCrMo3, and 34CrNiMo6 harden well even in large sections. They are often purchased already heat-treated (+QT), with a yield strength (Rm) of around 900–1100 N/mm², and are machined directly in that condition.

Case-hardening steels

They have a low carbon content (0.10–0.25%): the core remains tough. During carburizing, the surface layer is enriched with carbon, which—after hardening—becomes extremely hard (approximately 58–62 HRC) and resistant to wear. Examples: C15E, 16MnCr5, 20MnCr5, 18CrNiMo7-6 (heavily loaded gears). They are machined before heat treatment; afterward, only grinding is required.

Nitriding Steels

They contain elements that form hard nitrides with nitrogen: aluminum, chromium, molybdenum, and vanadium. Nitriding is performed at a relatively low temperature (about 500 °C) and causes very little distortion of the workpiece, which can therefore be finished before the treatment. Examples: 41CrAlMo7-10, 31CrMoV9; 42CrMo4 also nitrides well.

Spring Steels

They must have very high yield strength to return to their original shape without deforming: medium-to-high carbon content, along with silicon, chromium, or vanadium. Examples: 51CrV4, 54SiCr6, C67S, and C75S for strips and flat springs.

Free-cutting steels

They are designed for automatic and multi-spindle lathes, where short chips that break off on their own are required. They contain high levels of sulfur (0.2–0.4%) and manganese, which form manganese sulfide inclusions: the chip breaks along these inclusions like a perforated sheet. Lead (11SMnPb37) further improves machinability. On the other hand, they have low toughness, should not be welded, and are not suitable for workpieces subject to high fatigue stress. There are also quenched and tempered free-cutting steels (for example, 36SMnPb14) and, due to environmental restrictions on lead, lead-free versions.

Steels for Bearings

100Cr6 contains 1% carbon and 1.5% chromium: when hardened, it reaches approximately 60–64 HRC and offers excellent resistance to contact fatigue. It is the steel used for ball bearings, roller bearings, and bearing rings, but it is also used for pins, guide pins, and gauges.

20.9 Stainless Steels

Steel is considered stainless when it contains at least 10.5% chromium (and no more than 1.2% carbon, according to the EN 10088 standard). When chromium comes into contact with oxygen in the air or water, it forms a layer of chromium oxide on the surface that is just a few nanometers thick, transparent, compact, and firmly bonded to the metal: the passive film. This film isolates the steel from the environment, and if it gets scratched, it reforms on its own. Stainless steel, therefore, is not “steel that does not rust”: it rusts immediately, but only on the surface, and the oxide protects it.

chromium oxide filma few nanometers thicksteel with Cr ≥ 10.5%1 · protectedoxygen in the air2 · scratchedthe film reformson its own in a few moments3 · repassivated
Figure 20.7 · The passive film (green, shown with greatly exaggerated thickness) protects stainless steel; a scratch breaks it, but oxygen rebuilds it. Free iron left behind by tools and brushes made of ordinary steel, on the other hand, rusts on top of the stainless steel.
FamilyTypical CompositionFeaturesExamples
AusteniticCr 17–19%, Ni 8–13%, low C; sometimes Mo 2–3%Non-magnetic, highly ductile and tough, with excellent corrosion resistance; they do not harden through heat treatment; they work-harden significantly under the toolX5CrNi18-10 (304), X2CrNiMo17-12-2 (316L), X8CrNiS18-9 (303, free-cutting)
FerriticCr 11–18%, low C, no Nimagnetic, inexpensive, moderate corrosion resistance; cannot be hardenedX6Cr17 (430)
MartensiticCr 12–18%, C from 0.1 to over 1%magnetic, they harden; lower corrosion resistanceX20Cr13 (420), X46Cr13 (knives, tools)
DuplexCr 22–25%, Ni 4–7%, Mo 3%, nitrogenHalf austenite, half ferrite: yield strength nearly double that of austenitic steels; excellent performance in seawater; difficult to machineX2CrNiMoN22-5-3 (1.4462)

Approximate values, rounded. The closest AISI designation is shown in parentheses.

Stainless steels are evaluated for resistance to pitting (small, deep craters caused by chlorides, such as salt) using a number called the PREN (Pitting Resistance Equivalent Number): the higher the number, the better the resistance.

Pockmark Resistance Index
PREN = Cr + 3.3 · Mo + 16 · N
Cr, Mo, N: mass percentages of chromium, molybdenum, and nitrogen. This is a comparative number with no units.
Example 20.11 · Which type of stainless steel should be used for a workpiece located near the sea?
304 (18% Cr, no Mo, negligible nitrogen): PREN = 18
316L (17% Cr, 2.2% Mo): PREN = 17 + 3.3 × 2.2 = 17 + 7.26 = 24.26
Duplex 1.4462 (22% Cr, 3.1% Mo, 0.17% N): PREN = 22 + 3.3 · 3.1 + 16 · 0.17 = 22 + 10.23 + 2.72 = 34.95
For marine environments, 316L is the minimum reasonable standard; for actual seawater, duplex is required
🔧
Machining austenitic stainless steel. Work hardening occurs: if the tool skids without cutting, the surface layer hardens, and the next pass encounters a harder material. Therefore, work with sharp cutting edges, using feeds and depths that are not too small, without any dwell time in contact with the material, and with ample coolant. For bar stock, the X8CrNiS18-9 (AISI 303) free-cutting steel is preferred, if the drawing allows it.

20.10 Tool Steels

Steels used for tools, dies, and molds must be hard, wear-resistant, and—depending on their application—maintain their hardness at high temperatures. They typically contain high levels of carbon and many carbide-forming elements. They are machined in the annealed (soft) state, then hardened, and finally finished by grinding or electrical discharge machining.

TypeExamplesApproximate Service HardnessUses
for cold machining operationsX153CrMoV12 (1.2379), 90MnCrV8 (1.2842)58–62 HRCblanking dies, punches, dies, shear blades, gauges
for hot machining operationsX40CrMoV5-1 (1.2344)44–52 HRCDie-casting and hot-forming molds: resistant to temperature fluctuations
for plastic molds40CrMnMo7 (1.2311)approximately 30 HRC, already heat-treatedInjection molds: They are milled as-is upon delivery
high-speed (HSS)HS6-5-2 (1.3343), HS6-5-2-5 (1.3243), HS2-9-1-8 (1.3247)63–66 HRCdrill bits, taps, end mills, hobs, broaches: they remain hard up to about 550–600 °C

Approximate values, rounded. Cobalt-based high-speed steels (those with a fourth digit) are more heat-resistant and are used for difficult materials such as stainless steel; versions made from sintered powders are more tough. A comparison with cemented carbide and other tool materials is provided in Chapter 25.

20.11 Commercial Forms and Their Masses

The steel arrives at the workshop as a semi-finished product in standard shapes and sizes. Knowing the shapes and their tolerances helps in choosing the right blank: too little allowance won’t clean the surface, while too much wastes time and material.

dtoandsbsDsroundsquarehexagonflattubeswidth × lengthsheet metalL-channelUPNIPE
Figure 20.8 · The most common cross-sections with their identifying dimensions. The hexagons are sorted by the dimension on the faces s (the key); the dimension on the edges e is 1.1547 · s.
  • Hot-rolled bars (round, square, flat, hexagonal): dark surface with rolling scale, wide tolerances. For a round bar with a diameter of Ø50, the tolerance is on the order of ±0.8 mm, plus ovality: an allowance for roughing must always be provided.
  • Cold-drawn bars (bright): tight tolerances, usually h9 for round bars and h11 for square, hexagonal, and flat bars (ISO tolerances are listed in Chapter 14). A Ø20 h9 drawn round bar measures between 19.948 and 20.000 mm. Work hardening makes them slightly stronger but introduces internal stresses.
  • Stripped bars (peeled on a lathe) and adjusted: free of surface defects; tolerances h10–h11 for turned parts, h6–h8 for ground parts (guide shafts, stems).
  • Sheet metal: hot-rolled (thicknesses of 1.5–2 mm and up, dark surface) or cold-rolled (thin thicknesses, smooth and glossy surface, for example, DC01). They are ordered by thickness × width × length, for example, 5 × 1000 × 2000.
  • Tubes: welded or seamless; they are designated by outer diameter × wall thickness (for example, 60.3 × 4). Cold-drawn precision tubes have tolerances of just a few hundredths.
  • Structural sections: IPE and HEA/HEB beams, C-channels (UPN), L-angle and T-angle sections: these are primarily used in structural steelwork and machine frames.

The bars are usually sold in lengths of 3 or 6 meters. To calculate their weight, use the mass per meter, as discussed in sections 2.14 and 4.10: cross-sectional area multiplied by density.

Mass per meter of steel products (ρ = 7.85 kg/dm³)
m′ = ρ · A1000
circle 0.006165 · d² · square 0.00785 · a² · hexagon 0.0068 · s²
plate 0.00785 · b · s · tube 0.02466 · s · (D − s)
m′ mass per meter in kg/m · ρ density in kg/dm³ · A cross-sectional area in mm² · d diameter, a side, s the length of the sides of the hexagon or its thickness, b width, D outer diameter of the tube, all in mm. For austenitic stainless steel (7.9 kg/dm³), multiply by 7.9 / 7.85.
Example 20.12 · How much does a round bar weigh?

A 3-meter-long C45 bar with a diameter of 60. How much does it weigh? Can it be lifted by hand?

area: A = π · 60² / 4 = 2,827.43 mm²
mass per meter: m′ = 7.85 × 2827.43 / 1000 = 22.195 kg/m (using the short formula: 0.006165 × 3600 = 22.19 kg/m)
whole bar: 22.195 × 3 = 66.59 kg
About 66.6 kg: too heavy for one person; you'll need a hoist or two people
Example 20.13 · Hexagon, Pipe, and Sheet Metal
32-hex key, 3-meter bar: m′ = 0.0068 · 32² = 6.96 kg/m → 6.96 · 3 = 20.88 kg; measurement along the edges e = 1.1547 × 32 = 36.95 mm
Pipe 60.3 × 4, 6 m long: m′ = 0.02466 · 4 · (60.3 − 4) = 0.02466 · 4 · 56.3 = 5.553 kg/m → 5.553 · 6 = 33.32 kg
sheet metal 5 × 1000 × 2000: volume 0.05 × 10 × 2000 = 10 dm³ → 10 × 7.85 = 78.5 kg
20.88 kg · 33.32 kg · 78.5 kg

20.12 Machinability on Machine Tools

Machinability indicates how easy it is to remove chips from a material: how long the cutting edge lasts, what forces are required, what kind of chips are formed, and what kind of surface finish is achieved. It is often expressed as a machinability index: a reference steel is set to 100, and other steels are compared based on the cutting speed that yields the same tool life. An index of 50 means, roughly speaking, half the cutting speed is required to wear down the cutting edge in the same amount of time.

For cutting tools, materials are divided into the ISO groups already shown in Table 26.12: P (blue) steels, including ferritic and martensitic stainless steels; M (yellow) austenitic and duplex stainless steels; K (red) cast irons; N: non-ferrous metals; S: superalloys and titanium; H: hardened materials. The group indicates which insert grade to choose (Chapter 25).

P · steelsM · austenitic and duplex stainless steelsK · cast iron11SMnPb37 (Pb-alloyed free-cutting steel)12011SMn30 (free-cutting)100C15, S235JR55Normalized C4540annealed 42CrMo44542CrMo4 quenched and tempered34100Cr6 annealed30X153CrMoV12 annealed20X8CrNiS18-9 (AISI 303)50X5CrNi18-10 (AISI 304)32X2CrNiMo17-12-2 (316L)27X2CrNiMoN22-5-3 (duplex)20EN-GJL-25050EN-GJS-400-1545EN-GJS-700-230reference = 100
Figure 20.9 · Indicative machinability index, with 11SMn30 as the reference (100). Rounded average values compiled by CNC Simulator Italia: these values vary depending on the condition of the material and the tool.

What makes a material easy or difficult to work with:

  • Hardness: the higher it is, the faster the cutting edge wears down; but even a material that is too soft (mild steel, C10) performs poorly, because it causes the metal to stick to the tool and form a built-up edge;
  • Toughness and work hardening: austenitic and duplex steels produce long, tough chips and harden under the tool;
  • the hard carbides in tools and the low thermal conductivity of stainless steels, which causes heat to remain at the cutting edge;
  • Sulfide and lead inclusions, which break up the chips and provide lubrication: that's why automatic machines rank at the top.
Cutting Speed Correction Using the Machinability Index (Estimate)
Vc2 ≈ Vc1 · I2I1
Vc1: Tested cutting speed on material 1 in m/min · Vc2: Speed to be tested on material 2 in m/min · I1, I2: Machinability indices. This serves as a starting point for materials of the same type, using the same tool; with modern carbide inserts, the differences are smaller than the index suggests.
Example 20.14 · Changing Materials Without Changing the Program at Random

A normalized C45 pin (index 40) turns well at Vc = 200 m/min. The same workpiece is to be made from quenched and tempered 42CrMo4 (index 34) and 304 stainless steel (index 32). What starting speed should be used?

Quenched and tempered 42CrMo4: Vc ≈ 200 · 34 / 40 = 170 m/min
304: Vc ≈ 200 × 32 / 40 = 160 m/min
Comparison with Table 26.12: 140–200 m/min for quenched and tempered alloy steels and 120–180 m/min for austenitic stainless steels during roughing: the estimated values fall within these ranges
Start at 170 and 160 m/min, then adjust based on the chips and wear (for stainless steel, also use an M-series insert)

20.13 Cast Iron

Cast irons contain 2.5 to 4% carbon and usually 1 to 3% silicon. In most machine cast irons, the carbon does not remain bound to the iron but separates as graphite—pure, soft, black carbon—dispersed throughout the metal matrix. It is the form of the graphite that determines the properties of the cast iron.

gray laminatelamellae: numerous internal groovesworm-likeshort, rounded wormsspheroidalspherical: no notches
Figure 20.10 · Diagram (not a photo): flake graphite creates many small notches and makes gray cast iron brittle under tensile stress; spheroidal graphite hardly weakens the matrix at all. In spheroidal graphite cast iron, the spheres are often surrounded by a ferrite halo.

Lamellar gray cast iron (EN-GJL)

Graphite consists of lamellae, which, when viewed in cross-section, resemble many small cracks. For this reason, gray cast iron has low tensile strength, no yield point, and breaks without elongation (A < 1%), while its compressive strength is three or four times greater (Chapter 10). On the other hand, it possesses valuable properties for tools:

  • It dampens vibrations much better than steel: the graphite flakes absorb energy with every runout;
  • It pours well into complex molds with ribs and cavities, and it's inexpensive;
  • It is easy to work with short, powdery chips, and the graphite acts as a lubricant: the cast-iron slideways glide smoothly;
  • It remains stable over time, especially after a stretching treatment.

For this reason, the bases, beds, columns, slides, and heads of tool machines have always been made of gray cast iron (and today also of ductile cast iron, welded steel, or polymer-modified concrete).

steelweldedgray cast ironEN-GJLtimetimesame impact at the start: in cast iron, the vibration dies out much sooner
Figure 20.11 · Qualitative vibration behavior after an impact: gray cast iron dampens vibrations many times more effectively than steel (roughly 5 to 10 times more, depending on the type).

Spheroidal graphite cast iron (EN-GJS)

By adding a small amount of magnesium to the melt, graphite forms in spherical particles. Without the lamellar structure, cast iron becomes strong and ductile, almost like steel: it has a yield strength, elongates by 2 to 18 percent depending on the type, and withstands impact and fatigue. It is used for crankshafts, hubs, valve bodies, supports, large gears, and water pipes. When specially treated (ADI, EN-GJS-800-10 and higher grades), it achieves the strength of alloy steel.

Malleable and vermicular cast iron

Malleable cast iron starts out white (with all the carbon bound as cementite, making it extremely hard and brittle) and becomes tough through a long annealing process that transforms the cementite into graphite nodules. It is used for small, thin-walled castings: fillets, handles, and chain parts. It is designated as EN-GJMW (white-heart) or EN-GJMB (black-heart). Vermicular cast iron (EN-GJV) contains graphite in the form of short worms: it falls midway between gray and spheroidal cast iron in terms of strength, thermal conductivity, and damping, and is used for diesel engine blocks, brake discs, and exhaust manifolds.

Designation of Cast Iron (EN 1561, EN 1563)

The designation always begins with EN-GJ: EN for European standard, G for cast, J for cast iron (from the English word iron; the letter I is not used because it can be confused with the number one). This is followed by the letter indicating the graphite structure: L for lamellar, S for spheroidal, M for malleable, V for vermicular. Then:

  • For gray cast iron (EN 1561), the minimum tensile strength in N/mm², measured on test specimens: EN-GJL-250 has Rm ≥ 250 N/mm²;
  • For spheroidal graphite cast iron (EN 1563) and malleable cast iron, two values are specified: minimum Rm and minimum elongation in %: EN-GJS-400-15 has Rm ≥ 400 N/mm² and A ≥ 15%.

Cast irons also have a designation that begins with EN-J: for example, EN-JL1040 corresponds to EN-GJL-250, and EN-JS1030 corresponds to EN-GJS-400-15. On older drawings, you can still find UNI designations such as G 25 (gray cast iron with a strength of 250 N/mm²) or GS 400-12.

Cast ironRe (N/mm²)Rm (N/mm²)A%E (N/mm²)Typical Uses
EN-GJL-200does not have200less than 1100 000covers, lids, small brackets
EN-GJL-250does not have250less than 1110 000machine tool bases and pallets
EN-GJL-300does not have300less than 1120 000Heavily loaded pallets, cylinders, brake discs
EN-GJS-400-1525040015170 000bearings, hubs, valve bodies
EN-GJS-500-73205007170 000levers, brackets, gears
EN-GJS-700-24207002175 000shafts, gears
EN-GJMB-350-1020035010170 000fillets, small, thin jets
EN-GJV-4002804001-2145 000engine mounts, manifolds

Approximate, average, and rounded values compiled by CNC Simulator Italia (consistent with Table 10.4). Density: approximately 7.2 kg/dm³ for gray cast iron, 7.1 kg/dm³ for ductile cast iron. In actual castings, strength depends on wall thickness.

Example 20.15 · Reading Cast Iron Designations and Weighing a Base
EN-GJL-250 → lamellar gray cast iron, Rm ≥ 250 N/mm²
EN-GJS-400-15 → ductile iron, Rm ≥ 400 N/mm², elongation ≥ 15%

A base has a metal volume of 0.25 m³ = 250 dm³. How much does it weigh when made of gray cast iron, and how much would it weigh if it were made of steel?

cast iron: 250 × 7.2 = 1,800 kg · steel: 250 × 7.85 = 1,962.5 kg
difference: (7.85 − 7.2) / 7.85 × 100 = 8.3%
For the same volume, cast iron weighs about 8% less; however, it has a lower E-modulus (110,000 vs. 210,000 N/mm²), so stronger cross-sections are needed to achieve the same stiffness

Steels for Casting

When a workpiece has a complex shape but must be as strong as steel (in terms of toughness, weldability, and impact resistance), steel is cast instead of cast iron. This is more difficult because steel melts at a higher temperature and shrinks more, but the result is castings that are weldable and tough: pump and valve bodies, hooks, levers, and wheels. The designation begins with G: GE240 (cast steel for mechanical applications, Re ≥ 240 N/mm²), G20Mn5 (cast steel, weldable), GX5CrNi19-10 (austenitic stainless steel for casting).

20.14 Choosing a Steel: Practical Examples

There is no such thing as the "best" steel; there is only the right steel for the workpiece. The questions to ask are always the same: How much load will it bear (and what kind: static, fatigue, or impact)? Does it need to withstand wear or corrosion? Does it need to be welded? Does it need to be heat-treated, and if so, before or after machining? How many workpieces are being produced, and on which machine? How much does the material cost, including machine time?

Example 20.16 · A shaft: C45 or 42CrMo4?

A torsion shaft made of quenched and tempered C45 steel (Re 490 N/mm²) has a diameter of 50. If made from quenched and tempered 42CrMo4 (Re 750 N/mm²), what would the diameter be, and how much would it cost per meter? Approximate prices: C45 €1.60/kg, quenched and tempered 42CrMo4 €2.40/kg.

For torsional stress, the diameter is related to the cube root of the allowable stress (Chapter 10), which is proportional to Re: d2 = 50 · ∛(490 / 750) = 50 · 0.8677 = 43.39 mm → a Ø45 bar is used
C45 Ø50: 0.006165 × 2,500 = 15.41 kg/m → 15.413 × 1.60 = 24.66 €/m
42CrMo4 Ø45: 0.006165 × 2025 = 12.48 kg/m → 12.48 × 2.40 = 29.95 €/m
Differences: mass −19.0%, material cost +21.5%
42CrMo4 results in smaller, lighter shafts (with smaller bearings and a smaller overall footprint) at a slightly higher material cost. If there is enough space, C45 is sufficient; if the shaft is large or subjected to high stress, 42CrMo4 hardens more thoroughly and is the better choice.
Example 20.17 · A High-Strength Screw

A Class 10.9 bolt is required (nominal Rm 1000 N/mm², Re = 0.9 × 1000 = 900 N/mm², Chapter 18). What type of steel should it be made of?

S235 or E295: The yield strength is one-fourth or one-third of the required value, and they cannot be reliably hardened → no
C45: After heat treatment, it reaches 10.9 only in small diameters → at the limit
Quenched and tempered 42CrMo4 (or boron steels suitable for quenching and tempering): For these screw diameters, the quenching and tempering process results in an Rm value exceeding 1000 N/mm² even at the core → yes
Quenched and tempered alloy steel, typically 42CrMo4 or a boron steel: this is what fastener manufacturers use for classes 10.9 and 12.9
Example 20.18 · A workpiece from an automatic lathe

A hexagonal fillet, size 24, 40 mm long, subject to low stress, to be produced in a batch of 10,000 workpieces on a sliding-head lathe. Cutting results in a 3 mm loss; the final segment of each 3-meter bar is 250 mm.

Material: 11SMnPb37 drawn lead-free steel H11: short chips, high speeds, excellent finishing; the workpiece is neither welded nor heavily loaded
workpieces per bar: (3000 − 250) / (40 + 3) = 2750 / 43 = 63.95 → 63 workpieces
Number of bars needed: 10,000 / 63 = 158.7 → 159 bars
mass per meter: 0.0068 × 24² = 3.917 kg/m → one bar weighs 3.917 × 3 = 11.75 kg; total material weight: 159 × 11.75 = 1,868 kg
Starting with a circle, to get a hexagon you would need a diameter of at least Ø 1.1547 × 24 = 27.71 mm, plus the milling of the faces: using a drawn hexagonal bar saves one step
11SMnPb37 hexagonal wire rod, 24, 159 bars (approximately 1.9 metric tons)
Example 20.19 · Three Workpieces, Three Choices
guide pin that slides in a bushing, with a tough core → case-hardened steel (16MnCr5), case-hardened and tempered to 58–62 HRC, ground to finish
Welded bracket on a frame, subject to low loads → S235JR or S355J2; if used in cold conditions or subject to higher loads: weld without preheating
Shaft of a saltwater pump → stainless steel: 316L minimum (PREN 24), duplex 1.4462 if the shaft is under load or the water is seawater (PREN 35, nearly double the yield strength)
First, you decide what the workpiece is supposed to do; then you choose the family; finally, you specify the exact part number that the supplier has in stock.
📦
The material that's available. Before writing down a rare custom-order drawing, it's best to check with the supplier: C45, 42CrMo4, 39NiCrMo3, 16MnCr5, 11SMnPb37, 304, and 316L in bar form are readily available everywhere; special-purpose steel, on the other hand, may involve a wait of several weeks and a minimum order quantity.

8:15 p.m. The Formulas in This Chapter

WhatFormula or rule
Perlite in carbon steel (estimate)perlite % ≈ C / 0.77 × 100 (C ≤ 0.77%)
Carbon in chemical formulasC % = initial number / 100
Elements in the bass parts% = number / factor (4: Cr, Co, Mn, Ni, Si, W · 10: Al, Be, Cu, Mo, Nb, Pb, Ta, Ti, V, Zr · 100: Ce, N, P, S · 1000: B)
High-leg (X) and rapid (HS)The figures are already percentages; HS: W-Mo-V-Co
Resistance to pittingPREN = Cr + 3.3 · Mo + 16 · N
Mass per meterm′ = ρ · A / 1000 (kg/m, A in mm², ρ in kg/dm³)
Steel Weights by the Metercircle 0.006165 d² · square 0.00785 a² · hexagon 0.0068 s² · flat 0.00785 b s · tube 0.02466 s (D − s)
Hexagon: Measurements Along the Edgese = 1,1547 · s
Cutting Speed and Machinability IndexVc2 ≈ Vc1 · I2 / I1

20.16 Exercises

Try to solve them on your own, using a calculator, before looking at the solution.

Exercise 1. What do the abbreviations S275J0, E360, C22E, and S355K2+N stand for?
Solution

S275J0: structural, Re ≥ 275 N/mm², 27 J at 0 °C. E360: mechanical engineering, Re ≥ 360 N/mm². C22E: unalloyed, 0.22% C, maximum specified sulfur content. S355K2+N: structural steel, yield strength (Re) ≥ 355 N/mm², impact energy 40 J at −20 °C, normalized.

Exercise 2. Calculate the carbon content and the content of the specified element for 34CrNiMo6, 16MnCr5, 100Cr6, and 31CrMoV9.
Solution

34CrNiMo6: 0.34% C, Cr = 6 / 4 = 1.5%, Ni and Mo present. 16MnCr5: 0.16% C, Mn = 5 / 4 = 1.25%, Cr present. 100Cr6: 1.00% C, Cr = 6 / 4 = 1.5%. 31CrMoV9: 0.31% C, Cr = 9 / 4 = 2.25%, Mo and V present.

Exercise 3. Write the designation for a steel with 0.20% C, 1.25% Mn, and 1.1% Cr (specify the manganese content only), and that for a tool steel with 0.40% C, 5% Cr, 1.3% Mo, and 1% V (specify the chromium and molybdenum content).
Solution

First: low-alloy steel, 0.20 × 100 = 20, Mn 1.25 × 4 = 5 → 20MnCr5. Second: the chromium content reaches 5%, so it is high-alloy: X, 40, Cr 5, Mo 1.3 → 1 → X40CrMoV5-1.

Exercise 4. To which family do the materials 1.4404, 1.3505, 1.0715, and 1.2379 belong?
Solution

1.4404: stainless steel with at least 2.5% nickel and molybdenum (X2CrNiMo17-12-2, 316L). 1.3505: bearing steel (100Cr6). 1.0715: non-alloy steel (11SMn30, free-cutting). 1.2379: alloy tool steel (X153CrMoV12).

Problem 5. How much does a 40 × 40 square bar that is 2.5 m long weigh? And how much does an 80 × 10 plate that is 6 m long weigh?
Solution

Frame: 0.00785 · 40² = 12.56 kg/m → 12.56 · 2.5 = 31.4 kg. Plate: 0.00785 · 80 · 10 = 6.28 kg/m → 6.28 · 6 = 37.68 kg.

Exercise 6. A tube measuring 48.3 × 3.2 and 6 m long: How much does it weigh?
Solution

m′ = 0.02466 · 3.2 · (48.3 − 3.2) = 0.02466 · 3.2 · 45.1 = 3.559 kg/m → 3.559 · 6 = 21.35 kg.

Exercise 7. Estimate the percentage of perlite in a slowly cooled C60.
Solution

0.60 / 0.77 × 100 = 77.9%, approximately 78% (using the exact formula: (0.60 − 0.02) / 0.75 × 100 = 77.3%).

Exercise 8. Calculate the PREN of the X2CrNiMoN22-5-3 duplex stainless steel with 22% Cr, 3% Mo, and 0.17% N, and compare it to that of 304.
Solution

PREN = 22 + 3.3 × 3 + 16 × 0.17 = 22 + 9.9 + 2.72 = 34.62, almost double 304 (18).

Exercise 9. A normalized C45 workpiece (hardness index 40) is machined at 200 m/min. What feed rate should be used for the same workpiece made of 316L (hardness index 27)?
Solution

Vc ≈ 200 · 27 / 40 = 135 m/min, which falls within the 120–180 m/min range specified in Table 26.12 for austenitic stainless steels; Group M insert.

Exercise 10. What do the designations EN-GJL-300, EN-GJS-600-3, and EN-GJMB-350-10 mean?
Solution

EN-GJL-300: lamellar gray cast iron, Rm ≥ 300 N/mm². EN-GJS-600-3: spheroidal cast iron, Rm ≥ 600 N/mm², A ≥ 3%. EN-GJMB-350-10: black-heart malleable cast iron, Rm ≥ 350 N/mm², A ≥ 10%.

Exercise 11. A 2-meter-long, Ø80 shaft made of 42CrMo4 steel, heat-treated, costing 2.40 €/kg: How much does it weigh, and how much does the blank cost?
Solution

m′ = 0.006165 × 80² = 39.46 kg/m; mass 39.46 × 2 = 78.92 kg; cost 78.92 × 2.40 = 189.41 €.

Exercise 12. 50 metric tons of cast iron containing 4.2% carbon are fed into a converter; the goal is to produce steel containing 0.45% carbon. How much carbon must be burned off?
Solution

50 · 0,042 − x = 0,0045 · (50 − x) → 2,1 − x = 0,225 − 0,0045x → 1,875 = 0,9955x → x = 1,883 t.

Exercise 13. Choose the appropriate steel (or cast iron) grade for: a heavily loaded gear with hardened teeth; a leaf spring; the base of a grinding machine; a blanking punch.
Solution

Gear: case-hardened steel, such as 18CrNiMo7-6 or 16MnCr5, case-hardened and tempered. Spring: spring steel, such as 51CrV4. Base: gray cast iron, such as EN-GJL-250, for vibration damping and stability. Punch: cold-machining tool steel, such as X153CrMoV12, hardened to 58–62 HRC.

Exercise 14. From 3-meter-long hexagonal bars with a 24 key, 25 mm-long workpieces are cut, with a 3 mm cut-off and a 250 mm end piece. How many workpieces per bar? What is the minimum diameter of a round bar needed to produce the hexagon?
Solution

(3000 − 250) / (25 + 3) = 2750 / 28 = 98.2 → 98 workpieces. Minimum diameter: 1.1547 × 24 = 27.71 mm, so in practice a Ø28 or Ø30.