Chapter 24

Metal Cutting

A lathe, a milling machine, and a drill are different machines, but the actual work is always done by the same thing: a hard wedge that penetrates the metal and cuts off a chip. In this chapter, we’ll take a close look at what happens within those few tenths of a millimeter: how the chip is formed, what the cutting edge angles are for, where the heat goes, why the tool wears out, and how to choose the speed that costs the least. The formulas for speed, force, and power in turning are in Chapter 26; here we explain the physics behind them.

24.1 What happens when you cut

Anyone watching a lathe in action might think that the cutting edge “slices” through the metal the way a knife slices through bread. That’s not the case. The cutting edge pushes a layer of material—the thick one—ahead of it h which must become chip, and it crush until the metal yields and begins to flow. The chip is the result of an extremely intense plastic deformation concentrated in a thin area, not of a blade cutting between two layers.

When viewed from the side under a microscope, the tip reveals three distinct zones where the metal is active (Figure 24.1):

  • the primary zone, or flow zone: a narrow band extending from the cutting edge to the free surface of the workpiece. Here, the metal deforms suddenly, flows over itself like a deck of cards pushed to one side, and becomes a chip. Most of the cutting energy is consumed here;
  • the secondary zone, along the flank of the tool (the surface over which the chip slides): the newly formed chip slides over it under strong pressure, and the layer in contact is further deformed and heated by friction. It is the hottest zone of all;
  • The tertiary zone, below the tool flank: even though the flank is inclined backward, it rubs slightly against the freshly machined surface, which rebounds elastically after the cutting edge passes over it. This is where flank wear originates (paragraph 24.8).
123hVcchiptoolworkpiece1 Primary zone: the metal flows along the sliding plane (red line)2 secondary zone: the chip is pressed against the tool face3 tertiary zone: the flank rubs against the freshly machined surface
Figure 24.1 · Side view of the cut. The workpiece advances toward the tool at a cutting speed Vc; the layer of thickness h is compressed, flows through zone 1, and is carried back onto the face as a chip.

To study this phenomenon, it is helpful to imagine the workpiece moving against a stationary tool: on a lathe, the workpiece rotates; in milling, the tool rotates; but from the cutting edge’s perspective, nothing changes. The only factor that matters is the relative motion between the cutting edge and the material—that is, the cutting speed Vc defined in Section 26.3.

24.2 The Orthogonal Cut: Tracing and Sliding Angle

The simplest case to study is the orthogonal cut: the cutting edge is straight and perpendicular to the cutting speed, and the chip exits perpendicular to the cutting edge, without deviating to the side. In this case, a cross-sectional drawing is sufficient to understand everything (Figure 24.2). This is similar to what happens on a lathe when the end of a thin tube is faced with a 90° cutting edge.

hh′φγαVcVtrsliding surfacechiptoolworkpiece
Figure 24.2 · Model of orthogonal cutting. The chip is thicker (h′) than the cut layer (h) and moves more slowly (Vtr instead of Vc). φ is the angle of the sliding plane; γ and α are the tool angles (Section 24.4).

The tracing ratio

When you measure a steel chip with a caliper, you find that it is thicker than the layer the tool removed: the metal, pressed against the tool face, shortens and thickens. The ratio of the two thicknesses is called the compression ratio λ. Since the volume of the metal does not change and the width of the chip remains nearly the same, if the chip is thicker, it must also be shorter—and therefore slower:

Cutting Ratio and Chip Speed
λ = h′h Vtr = Vcλ
λ—trace ratio, a pure number, always greater than 1 (for steels, typically from 1.5 to 4) · h—thickness of the undeformed chip, in mm (on a lathe, h = f · sin κr, paragraph 26.6) · h′ measured chip thickness, in mm · Vc cutting speed in m/min · Vtr speed at which the chip flows over the face, in m/min

The sliding angle

The primary zone can be thought of as a sliding plane inclined at an angle φ relative to the cutting direction. The smaller φ is, the longer the plane is and the more metal must be slid: this requires more force and more energy, and the chip is often thick and compacted. A good cut has a large φ and a small λ. From the geometry shown in Figure 24.2, we can derive:

Sliding angle (orthogonal section)
tan φ = cos γλ − sin γ
φ: angle of the sliding plane relative to the cutting direction · γ: upper rake angle of the tool (Section 24.4) · λ: relief ratio. For steels, φ is usually between 15° and 35°.
Example 24.1 · Tracing and Sliding Angle

In an orthogonal cutting test on mild steel, the cut layer is h = 0.25 mm thick. The chip, measured with a micrometer, is 0.75 mm thick. The tool has γ = 6°. Find λ and φ.

λ = 0,750,25 = 3
cos 6° = 0.9945; sin 6° = 0.1045
tan φ = 0,99453 − 0,1045 = 0,99452,8955 = 0,3435
φ = arctan 0.3435 = 18.96°
λ = 3 and φ ≈ 19°: very tightly wound chip, typical of mild steel at low speeds
Example 24.2 · How fast does the chip move?

In the test described in Example 24.1, the workpiece moves against the cutting edge at Vc = 200 m/min. At what speed does the chip slide along the rake face?

Vtr = 2003 = 66.7 m/min
Vtr ≈ 67 m/min: The chips exit three times slower than the metal entering

With a more positive rake angle (larger γ) or a higher cutting speed, the chip is produced thinner and exits faster: λ decreases toward 2 and φ increases. This is one of the reasons why inserts for aluminum have a very positive rake angle.

24.3 Chip Types and the Cutting Edge

The same tool produces very different chips when used on different materials or with different parameters. Examining the chip is the first check a good lathe operator performs: it indicates whether the material, speed, feed, and angles are working well together. There are four distinct types (Figure 24.3).

continuous ribbon-like, smooth segmented sawtooth discontinuous fragmented with cutting edge with a built-up cutting edge
Figure 24.3 · The four types of chips. In the last drawing, the metal that has welded itself to the tip and the fragments it leaves on the surface are shown in red.
  • Continuous chip. A smooth chip on the face side and a slightly flaky chip on the other side. It is produced from ductile materials (steel, aluminum, copper) machined at medium and high speeds with a positive rake angle. It produces good surface finishes, but a long chip can wrap around the workpiece and the tool, posing a hazard; it must be broken up (section 24.14).
  • Segmented chip (or laminar, sawtooth). The flow is not uniform but jerky: the metal heats up in thin strips, where it becomes softer and flows suddenly. This is typical of titanium, superalloys, hardened steels, and—at very high cutting speeds—even ordinary steels. It causes the cutting force to vary from segment to segment and can trigger vibrations.
  • Intermittent chip formation (or in fragments). The metal breaks as soon as it begins to flow, and the chips come out in small pieces. This occurs with brittle materials, such as gray cast iron and certain types of brass, as well as with free-cutting steels containing sulfur and lead, which are specifically designed for this purpose (Chapter 20). It is easy to dispose of; with brittle materials, the surface is somewhat dull but smooth.
  • Chip with a built-up cutting edge. A small amount of metal is welded onto the tip and functions in place of the actual cutting edge. This is the most damaging of the four cases and deserves a separate discussion.

The cutting edge

In the secondary zone, the pressure between the chip and the faceplate is extremely high, and the surface of the chip is clean, freshly formed, and free of oxides. If the temperature is not high enough, the metal in the chip it is cold-welded on the chest, layer by layer, forming a small, hard, hardened lump: the replacement cutting edge (in English built-up edge, BUE). The chip grows until it becomes unstable, then breaks off: one workpiece is carried away with the chip, while another remains stuck to the machined surface. Then it begins to grow again.

welded cutting edgemetal workpiece welded to the chestfragments adhered to the surfacechiptoolThe deposit grows, breaks off, and grows back:dimensions and roughness fluctuate
Figure 24.4 · The cutting edge changes the shape of the tip: it cuts at a different angle and achieves deeper cuts, and when it breaks off, it carries away particles of the insert or leaves hard fragments on the workpiece.

There are three types of damage: the roughness worsens very (the surface is torn, with fragments glued back on), the The dimension is not stable because the actual cutting edge is constantly changing, and when the coating peels off, it can carry away small workpieces of the coating or the cutting edge (adhesion wear). This occurs mainly:

  • with soft, sticky materials: low-carbon steels, austenitic stainless steels, pure aluminum and soft aluminum alloys, copper;
  • at low cutting speeds, when the chip is not hot enough to soften and slide (for steel with carbide, generally below 60–80 m/min);
  • with a slightly positive or negative chest, cutting edges, and rough chest surfaces.

To prevent this, increase the cutting speed (this is the most effective remedy: above a certain temperature, the built-up edge no longer forms), use a more positive rake angle and a sharp, polished cutting edge, choose a coating with low chemical affinity for that material, and use a coolant with good lubricating properties. When drilling and tapping—where the speed at the center is necessarily low—the focus is primarily on the lubricant and geometry.

24.4 The cutting edge and its angles in cross-section

Any cutting tool—from a twist drill to a milling cutter, from a lathe insert to an engraver’s bur—is a wedge. It has two faces that meet at the cutting edge:

  • the face (upper cutting surface), over which the chip flows;
  • the flank (lower cutting edge), facing the surface that has just been machined.

Angles are measured in a section perpendicular to the cutting edge, relative to two reference planes: the cutting plane, which contains the cutting speed, and the reference plane, which is perpendicular to the cutting speed. The two planes are perpendicular to each other, so the three angles of the tool, when placed side by side, always form a right angle (Figure 24.5):

  • upper rake angle γ (gamma): between the chest and the reference plane;
  • cutting angle β (beta), or wedge angle: between the rake face and the flank, it is the “body” of the cutting edge;
  • Lower rake angle α (alpha): the angle between the flank and the cutting plane, that is, the machined surface.
γαβchesthipreferencecutting planeVcα + β + γ = 90°γ upper rake angleβ cutting angleα lower rake angle
Figure 24.5 · Angles in a cross-section perpendicular to the cutting edge. The vertical dashed line is the reference plane; the machined surface is the cutting plane. Drawing with γ = 12°, β = 70°, α = 8°.
Sum of the angles of the cutting edge
α + β + γ = 90° , so β = 90° − α − γ
α lower rake angle · β cutting angle · γ upper rake angle, all in degrees. γ can be negative: the face is inclined forward, and β becomes greater than 90° − α.
Example 24.3 · Cutting Angles of Two Tools

An HSS tool for mild steel is sharpened with α = 7° and γ = 12°. A negative insert for cast iron, mounted on the tool holder, operates with α = 6° and γ = −6°. What is the value of β in both cases?

HSS: β = 90° − 7° − 12° = 71°
negative insert: β = 90° − 6° − (−6°) = 90° − 6° + 6° = 90°
β = 71° for the HSS, β = 90° for the negative insert: a much more robust wedge

A “negative” insert is a plate with faces at 90° (β = 90°, no rake angle on the workpiece alone): the lower rake angle is created by tilting the insert in the tool holder, which is why the face is negative. In return, both sides of the insert can be used.

What is each corner used for?

The upper rake angle γ determines how easily the chip breaks away. A very positive front angle results in a “smooth” cut: the chip length is shorter (larger φ), forces and heat decrease, and the chip is thin. However, the chip becomes thin and brittle. A negative rake angle does the opposite: it generates more force and heat, but produces an extremely robust cutting edge that withstands impacts, built-up edge, interrupted cuts, and hard materials. Typical values: 15° to 25° for aluminum, 6° to 15° for steel with HSS or positive inserts, 0° to 8° for cast iron, and negative angles (−6° to −15°, often with a chamfer on the cutting edge) for hardened steels, ceramics, and CBN.

The lower rake angle α ensures that the flank passes through without scraping. If it is too small, the flank scrapes, heats up, wears out quickly, and can cause vibration; if it is too large, the wedge weakens. It is usually between 5° and 12°: less for hard materials, more for plastics and aluminum.

The cutting angle β isn't chosen arbitrarily: it's the one that remains. A large β means a sturdy cutting edge and a good heat dissipation path; a small β means a sharp but delicate cutting edge.

24.5 Plan Angles, Inclination, and Nose Radius

The angles in the cross-section describe the shape of the wedge. Three other angles describe the orientation of the cutting edge relative to the workpiece, as viewed from above, and one final value describes the shape of the tip.

Registration angle κr and tip angle εr

The rake angle κr (kappa) is the angle between the primary cutting edge and the feed direction, as previously used in Section 26.6 for the chip thickness h = f · sin κr. The secondary cutting edge forms the secondary rake angle κr′ with the machined surface, and between the two cutting edges lies the point angle εr (epsilon), which for inserts corresponds to the shape of the insert: 35° and 55° for profiling rhombuses, 60° for triangles, 80° for roughing rhombuses, and 90° for squares. The three angles lie on a straight line (Figure 24.6):

Angles in a floor plan
κr + εr + κr′ = 180°
κr clearance angle (determined by the tool holder) · εr point angle (determined by the shape of the insert) · κr′ secondary clearance angle, which must remain positive so that the secondary cutting edge does not scrape against the workpiece. All in degrees.
κrκr′εrprimary cutting edgesecondary cutting edgeapfeedrεenlarged tip
Figure 24.6 · The cutting edge viewed from above (drawing with κr = 75°, εr = 80°, κr′ = 25°). The chip section is shown in red. The circled area shows a magnified view of the tip: the edge is replaced by an arc of radius rε.
Example 24.4 · Is the secondary angle enough?

An 80° rhomboid insert is mounted on a tool holder with κr = 95°. On a profiling tool holder with κr = 93°, a 60° triangular insert is mounted instead. What is the value of κr′ in both cases?

80° rhombus: κr′ = 180° − 95° − 80° = 5°
60° triangle: κr′ = 180° − 93° − 60° = 27°
5° for the rhombus: it can rough-cut 90° shoulders but cannot copy on an incline; 27° for the triangle: it leaves room for profiling

With κr′ = 5°, even a small upward section of the profile is enough for the secondary cutting edge to touch the workpiece. To copy profiles with upward sections, sharper inserts (55° or 35°) are used, which result in a larger κr′.

What changes with κr? For a given feed rate, a small κr (45°–75°) distributes the chip over a longer cutting edge and makes it thinner: the feed rate can be increased, the cutting edge enters the workpiece gradually, and it withstands built-up edge better. In return, the radial force increases, causing long, thin workpieces to bend (section 24.6). A κr of 90°–95° applies force almost exclusively along the axis: this is the choice for straight shoulders and for workpieces with low rigidity.

Angle of inclination λs

The rake angle λs (lambda) is the angle of inclination of the primary cutting edge relative to the reference plane, as viewed from the front of the cutting edge (Figure 24.7). If λs = 0, the cut is orthogonal; if λs is nonzero, the cut is oblique, and the chip, instead of exiting perpendicular to the cutting edge, is deflected to the side by an angle approximately equal to λs.

  • With a negative λs, the tip is the lowest point of the cutting edge: initial contact with the material occurs in an area away from the tip—which is more robust—and the chip is pushed toward the workpiece. This is the preferred choice for roughing and interrupted cuts (negative inserts operate at approximately −6°);
  • When λs is positive, the tip is the highest point: the chip is removed from the machined surface and does not scratch it. This is the preferred choice for finishing and for thin workpieces.
λsFirst contactVctipNegative λs: the tip is the lowest pointview looking at the cutting edge from the frontcutting edgecutorthogonaloblique cut:the chip is deflectedthe rake face as seen from abovechip exit direction
Figure 24.7 · On the left, a front view of the cutting edge with a negative λs: the material, moving downward at Vc, first contacts the upper part, away from the tip. On the right, a top view of the rake face: in an oblique cut, the chip exits at an angle.

Nose radius rε

The tip is never a sharp edge: it is rounded with an arc, the nose radius rε, which for inserts is usually 0.2, 0.4, 0.8, 1.2, or 1.6 mm. A large nose radius makes the tip more robust and, for a given feed rate, produces a better surface finish (the formula for theoretical surface roughness is in Section 26.10); however, it increases the radial force and the tendency to vibrate. A small radius is used for light cuts, thin workpieces, and sharp internal edges. A rule of thumb: the depth of each pass should be at least about 2/3 of the nose radius; otherwise, only the arc is machined and the chip forms poorly.

MagnitudeIf it is large (or positive)If it is small (or negative)
γ upper shellsmooth cut, less force and heat, fragile cutting edgecutting edge and sturdy, with more power and warmth
α lower surfaceNo slippage, weak wedgeside-to-side rubbing, side wear, vibrations
κr recording(90°–95°) low radial force, thick chips(45°–75°) fine chip, gradual entry, more radial force
εr is the vertex anglesturdy bit, for rough cuttingthin tip, for contouring
λs inclinationchip away from the workpiece, to finishProtected tip, for roughing and interrupted cuts
r = nose radiussturdy tip, better roughness, more vibrationsless radial force, for gentle passes

Guidance table: The tool supplier specifies the correct values for each material. See Chapter 25 for information on selecting inserts and tool holders.

24.6 Shear forces and specific pressure

As the tool removes the chip, it experiences a resultant force from the workpiece that is inclined in space. As discussed in Chapter 8 (Figure 8.5), this force can be broken down into three components:

  • the shear force Fc, in the direction of the cutting speed: it is the largest and is used to calculate power;
  • the forward force Ff, acting against forward motion: the sled overcomes it;
  • The passive force Fp, which acts radially, pushes the tool away from the workpiece and bends it.

The method for calculating Fc using specific pressure—Fc = kc · ap · f—the table of values for kc1 and mc, and the power calculation are described in Section 26.9, along with Example 26.10. Here, we will examine where these forces come from and what they depend on.

How κr divides the thrust

In addition to Fc, which pushes “downward” on the chest, the chip exerts a force on the cutting edge that is perpendicular to the cutting edge itself, in the feed plane: let’s call this Fn. The rake angle determines how Fn is distributed between the feed direction and the radial direction (Figure 24.8). Neglecting the nose radius:

Feed Force and Passive Force (Estimate Without Nose Radius)
Ff = Fn · sin κr Fp = Fn · cos κr
Fn chip force perpendicular to the cutting edge, in the feed plane, in N · Ff forward thrust in N · Fp passive force (radial) in N · κr angle of incidence. In reality, the nose radius always adds a little radial force, even at κr = 90°.
feedFn = Ff = 800 NFp ≈ 0κr = 90°feedFn = 800 NFf = 566 NFp = 566 Nκr = 45°
Figure 24.8 · Top view: The thrust Fn is perpendicular to the cutting edge. When κr = 90°, the entire force acts along the workpiece axis; when κr = 45°, half of the force acts outward, in the radial direction.
Example 24.5 · How far does the cutting edge protrude?

The chip exerts a force of Fn = 800 N on the cutting edge. How is the thrust distributed when κr = 90°, 60°, and 45°?

κr = 90°: Ff = 800 · sin 90° = 800 N; Fp = 800 · cos 90° = 0 N
κr = 60°: Ff = 800 · 0,8660 = 692,8 N ; Fp = 800 · 0,5 = 400 N
κr = 45°: Ff = Fp = 800 · 0,7071 = 565,7 N
As the angle changes from 90° to 45°, the radial force changes from nearly zero to over 560 N

For a long, slender shaft that bends under radial force, a tool holder with κr close to 90° and a small nose radius is therefore selected.

What determines specific pressure?

The specific pressure kc is the shear force per square millimeter of the chip's cross-sectional area. It also has another very useful meaning: since N/mm² = N·mm/mm³, kc is also the energy required to turn one cubic millimeter of metal into a chip, expressed in thousandths of a joule. A kc value of 2500 N/mm² means 2.5 J per mm³, or 2500 J per cm³ of chip. It depends on:

  • the material: the more resistant and tough it is, the higher the value (this is the kc1 value in Table 26.9);
  • The chip thickness h: the thinner the chip, the greater kc becomes, according to kc = kc1 / hmc. The physical reason is that the cutting edge is never perfectly sharp: its slight rounding compresses and abrades a dimension of material that accounts for a larger proportion of the total when the chip is thin;
  • the upper rake angle γ: a more positive value reduces kc, while a negative value increases it. Rule of thumb: approximately 1% for every degree of difference from the γ value for which the table applies;
  • Cutting speed: only slightly. When you increase it, the chip heats up, becomes softer, and kc decreases slightly until it stabilizes;
  • Wear: A worn cutting edge creates more friction, and kc increases—even by several tens of percent toward the end of its service life.
Approximate correction for the upper rake angle
kc,γ ≈ kc · (1 − γ − γ0100)
kc specific pressure calculated as described in paragraph 26.9, in N/mm² · γ upper rake angle of the tool, in degrees · γ0 angle for which the table values apply (often about 6° for steels) · kc,γ correct specific pressure. This is a preliminary estimate.
Example 24.6 · Negative or Positive Insert

In Example 26.10, the specific pressure on C45 is kc = 2548 N/mm², using table data valid for γ0 = 6°. What are the values for a negative insert operating at γ = −6° and a positive insert at γ = 12°? And what is the shearing force, given ap = 3 mm and f = 0.25 mm/revolution?

γ = −6°: kc ≈ 2548 · (1 − (−6 − 6) / 100) = 2548 · 1.12 = 2853.8 N/mm²
Fc = 2853,8 · 3 · 0,25 = 2140 N
γ = 12°: kc ≈ 2548 · (1 − (12 − 6) / 100) = 2548 · 0.94 = 2395.1 N/mm²
Fc = 2395,1 · 3 · 0,25 = 1796 N
From 1,796 N (positive) to 2,140 N (negative): approximately 19% more force and power

24.7 Heat in the Cut

Almost all of the energy expended during cutting—more than 95%—is converted into heat: in the primary zone due to plastic deformation, and in the secondary and tertiary zones due to friction. The cutting power Pc mentioned in paragraph 26.9 is therefore, in practice, the thermal power generated at the cutting edge. The heat is distributed among the chip, the tool, and the workpiece in proportions that vary with speed: the faster the cutting speed, the more heat is carried away by the chip, because it escapes before the heat has time to transfer to the tool or the workpiece.

Where Does the Heat Go?Medium and high speedsWhat does it entail?
in the chips75-80%very hot, often colored chips; they must be removed
in the tool10-15%A small percentage, but concentrated in just a few mm³: that's what the cutting edge consumes
in the workpiece5-10%expansion and dimensions that change as the workpiece cools

Approximate breakdown for steel machined with carbide. At low speeds, the dimensions of the workpiece and the tool increase.

The typical temperatures during steel cutting with carbide tools, at normal cutting speeds, are 700–1,000 °C at the cutting face, where the chip passes, a few hundred degrees in the chip, and a few tens of degrees in the workpiece. This is why the tool material must remain hard at high temperatures: high-speed steel (HSS) begins to lose hardness above about 550–600 °C, cemented carbide withstands temperatures up to about 1000 °C, and ceramics and CBN even higher (Chapter 25). Austenitic stainless steels, titanium, and superalloys are poor heat conductors: the chip carries away less heat, and the cutting edge heats up more—one of the reasons they are machined more slowly.

Estimated Average Chip Temperature Rise
ΔT ≈ ηtr · kcρ · c
ΔT Average increase in chip temperature in °C (or K) · ηtr dimension of heat that goes into the chip (approximately 0.75–0.8) · kc specific pressure in N/mm², which is equal to J/cm³ · ρ density in g/cm³ · c specific heat in J/(g·K). This is calculated by stating that the energy per 1 cm³ of chips, kc joule heats that cm³ of metal.
Example 24.7 · Where Do the 6.37 kW from Example 26.10 Go?

In Example 26.10, the machining of C45 absorbs Pc = 6.37 kW with kc = 2548 N/mm². Let’s assume that 80% of the heat is in the chip, 10% in the tool, and 10% in the workpiece. How much thermal power goes where, and by how much does the chip heat up on average? For steel, ρ = 7.85 g/cm³ and c = 0.46 J/(g·K).

chip: 0.8 × 6.37 = 5.10 kW; tool: 0.1 × 6.37 = 0.64 kW; workpiece: 0.64 kW
energy per cm³ of chip: kc = 2548 N/mm² = 2548 J/cm³
ρ · c = 7.85 · 0.46 = 3.611 J/(cm³·K)
ΔT ≈ 0,8 · 25483,611 = 2038,43,611 = 564,5 °C
More than 5 kW in the chip, with about 640 W concentrated at the tip; the chip heats up to an average of over 500 °C

This is an overestimate: the specific heat of steel increases with temperature, and the chip begins to cool immediately. But the order of magnitude is correct, and that is why steel chips come out bluish: the color is due to a thin layer of oxide that forms above 250–300 °C. Note also that 640 W—the equivalent of a small electric stove—is concentrated within just a few cubic millimeters of the insert.

24.8 Tool Wear and Breakage

A cutting edge operates at hundreds of degrees, under pressures of thousands of newtons per square millimeter, with clean, hot metal sliding over it at meters per second. It can’t last forever. There are four mechanisms that wear it down, and they usually act together:

  • abrasion: Hard particles on the workpiece (carbides, oxides, foundry sand on scale) scratch the cutting edge like sandpaper. This is the predominant form of wear at low and medium speeds;
  • welding: micro-welds between the chip and the tool that, when they break away, carry away particles from the cutting edge (the same phenomenon as with a built-up edge);
  • Diffusion: At high temperatures, atoms from the tool (in the case of cemented carbide, primarily carbon and cobalt) migrate into the chip, which carries them away. This process dominates at high speeds and is the main cause of cratering;
  • oxidation and chemical reactions at the edges of the contact zone, where air enters.

Forms of Usury

When viewed through a magnifying glass, various forms of wear can be identified, each with its own cause (Figure 24.9 and table):

crater (KT)chipsnotchthe chest, viewed from abovelower cutting edgeVBcut at the ap dimensiontip wearcutting edgethe flank, front viewnew profile (hatched)plastic deformationthe hot cutting edge yields and sags
Figure 24.9 · The most common types of wear. VB is the width of the worn groove on the flank; KT is the depth of the crater on the root face. Schematic drawings showing exaggerated wear.
Form of wear and tearHow to Recognize ItMain causeRemedies
Sidewall wear (VB)a smooth, even band beneath the cutting edgeabrasion; this is “normal” wear and tearIf it's too fast: lower Vc, more wear-resistant quality
crater (KT)a hollow on the chest, just behind the cutting edgespread and excessively high temperature on the chestLower Vc or f values, alumina coating, more positive chest
carvingdeep notch on the cutting edge, at the dimension of the workpiece surfacehard crust, work hardening (stainless steel, superalloys), oxidationchange top with each pass, κr smaller, round insert
plastic deformationIf the tip is lowered or bulging, the workpiece will be out of dimensionTemperature and pressure are too high: the cutting edge failsLower Vc and f values, harder quality (less cobalt), cooling
chipssmall cracks along the cutting edgeimpacts, vibrations, interrupted cuts, cutting edge too brittlegreater toughness, chamfers or rounding of the cutting edge, greater rigidity
thermal cracksthin, comb-like cracks perpendicular to the cutting edgeAlternating heating and cooling (milling, intermittent coolant)Dry machining or machining with abundant, continuous coolant; higher toughness
breakThe tip or half-insert comes offoverload, wear that has been allowed to become excessive, impactReplace the cutting edge in a timely manner, reduce f and ap, use a more durable insert
⚠️
Don’t wait until it breaks. A cutting edge that breaks almost always damages both the tool holder and the workpiece, and chips that get lodged can ruin the turret. “Normal” wear is slow and predictable: even wear on the flank and a small crater. Any other type of wear is a sign that something needs to be corrected.

24.9 Wear Curves and Cutting Edge Life

Flank wear is the most consistent and easiest to measure; for this reason, it is used to determine when a cutting edge has reached the end of its service life. By measuring VB at regular intervals during a constant-speed test, a wear curve with three segments is obtained (Figure 24.10):

  • I · Break-in: In the first few minutes, the new, sharp edge rounds out, and VB improves rapidly;
  • II · Normal wear: a long, nearly straight section in which VB increases at a constant rate. This represents the service life of the cutting edge;
  • III · Accelerated wear: The tire is now wide, and the sidewall rubs, heats up, and wears down faster and faster. This increases the risk of a blowout.
510152025300.10.20.30.40.50T = 20.3T = 8.5End of life VB = 0.3 mmLowest VcHighest VcIII: even wearIII acceleratedCutting time t (min)VB (mm)
Figure 24.10 · Flank wear over time for two cutting speeds. The service life T is the time it takes for VB to reach the value selected as the end of life. At higher speeds, all three segments become shorter.

The most commonly used end-of-life criterion is a flank wear band width VB = 0.3 mm (standardized durability tests use this value as the average across the cutting edge). In practice, this is reduced to 0.1–0.2 mm for tight finishing operations, where dimensions and roughness are critical, and increases to 0.5–0.6 mm for heavy roughing. Other criteria are also used: crater depth, surface roughness outside tolerance limits, dimension deviation, increased power consumption, and chips that change color or shape.

The service life of the T-cutting edge is the actual cutting time, in minutes, required to reach the end-of-life criterion. Note: This is cutting time, not machine time. Rapid movements, tool changes, and workpiece loading do not wear down the cutting edge.

Example 24.8 · How long does the cutting edge last?

In a test on C45, the cutting edge reaches VB = 0.08 mm after a 2-minute break-in period. After that, wear increases steadily by 0.012 mm per minute. How long does it take to reach VB = 0.3 mm?

Wear to be accounted for in the regular section: 0.3 − 0.08 = 0.22 mm
Time on the regular section: 0,220,012 = 18.33 min
T = 2 + 18.33 = 20.33 min
T ≈ 20 minutes of cutting: this is the red curve in Figure 24.10

24.10 Taylor's Law

Of all the parameters, cutting speed has the greatest impact on the life of the cutting edge. In the early 20th century, the American engineer F. W. Taylor, after conducting thousands of tests, found that tool life and cutting speed are related by a simple law, which bears his name and is still used today (we have already encountered it in Example 1.24 and in Section 7.7):

Taylor's Law
Vc · T n = C
T = (CVc)1/n Vc = CT n T2T1 = (V1V2)1/n
Vc: cutting speed in m/min · T: cutting edge life in minutes of cutting · n: Taylor exponent, a pure number that depends primarily on the tool material · C: constant in m/min—this is the speed at which the cutting edge would last 1 minute. C depends on the workpiece material, tool, feed rate, depth of cut, and end-of-life criterion: it applies only under those conditions.
Tool Materialn (indicative)What does that mean?
high-speed steel (HSS)0,10-0,15The runtime drops sharply as soon as the speed increases
hard metal (including coated)0,20-0,300.25 is often used in calculations
ceramics0,40-0,60It handles high speeds well

Approximate values, rounded, for steel machining operations. Actual values require testing or data from the supplier.

On a bilogarithmic graph (Section 7.7), Taylor’s law is a straight line: log Vc = log C − n · log T. The slope of the line is −n. The flatter the line (small n), the more the service life is affected by speed: with the HSS, it doesn’t take much to wear out the cutting edge.

12510205010020501002005001,0002,000ceramic, n ≈ 0.5hard metal, n ≈ 0.25HSS, n ≈ 0.125Cutting edge life T (min), logarithmic scaleVc (m/min), logarithmic scale
Figure 24.11 · Indicative Taylor lines for three tool materials on the same steel. The larger n is, the steeper the line and the better the material withstands the increase in speed. The marked lines indicate the start of each decade.
Example 24.9 · Find n and C from two experiments

Using a carbide-tipped steel insert, two tests are conducted up to VB = 0.3 mm: at 260 m/min, the cutting edge lasts 8 minutes; at 170 m/min, it lasts 45 minutes. Find n and C.

260 · 8n = 170 · 45n → (45 / 8)n = 260 / 170
n = log (260 / 170)log (45 / 8) = log 1.5294log 5.625 = 0,184520,75012 = 0,2460
C = 260 × 80.2460 = 260 × 1.6678 = 433.6 m/min
check: 170 · 450.2460 = 433.6 ✓
n ≈ 0.25 and C ≈ 434 m/min: typical values for cemented carbide
Example 24.10 · Duration at a Different Speed, Speed for a Desired Duration

Using the straight line from Example 24.9 (n = 0.246, C = 433.6), how long will the cutting edge last at 220 m/min? And what speed must be used for it to last 30 minutes?

T = (433.6 / 220)¹/⁰.₂₄ 6 = 1.97114 0.065 = 15.8 min
300.246 = 2.3087 → Vc = 433.6 / 2.3087 = 187.8 m/min
At 220 m/min, it takes about 16 minutes; to extend the time to 30 minutes, the speed is reduced to about 188 m/min

The two speeds fall within the test range: these are reliable readings. Using the law far outside the tested range is risky, because at very low or very high speeds, the wear mechanisms change.

Example 24.11 · How Many Inserts for a Batch

A 4-edge insert, with n = 0.25 and C = 430 m/min, operates at 200 m/min. Each workpiece requires 1.8 minutes of cutting time. How many inserts are needed for a batch of 500 workpieces, assuming the cutting edge is always changed at the end of each workpiece?

T = (430 / 200)⁴ = 2.154 = 21.37 min
workpieces for cutting edges = 21.37 / 1.8 = 11.87 → round down: 11 workpieces
cutting edges = 500 / 11 = 45.45 → 46 cutting edges
inserts = 46 / 4 = 11.5 → 12 inserts
12 inserts; the cutting edge can be programmed to be replaced every 11 workpieces in the control unit's counter

The workpieces for cutting edges are rounded by default (the twelfth workpiece would end up with the cutting edge extending beyond the limit), the cutting edges and inserts by excess. According to the same law, at 250 m/min, the cutting edge would last (430 / 250)4 = 1,724 = 8.75 minutes: only 4 workpieces per cutting edge.

Taylor's Extended Law

The simple rule applies to fixed feed and depth. If these also change, an extended form is used, in which they appear with their exponents:

Extended Taylor's Law (brief overview)
Vc · T n · f a · ap b = C1
f: feed rate in mm/revolution · ap: cutting depth in mm · a, b: exponents, pure numbers: typically a ranges from 0.3 to 0.6 and b from 0.1 to 0.2 · C1: constant. Since n is smaller than a and a is greater than b, the duration is very sensitive to speed, less sensitive to feeds, and only slightly sensitive to depth.
Example 24.12 · Should you increase the feed rate or the speed?

We are machining at Vc = 200 m/min and f = 0.25 mm/rev. We want to increase the feed to 0.35 mm/rev without changing the cutting edge life. With a = 0.4, to what speed must we reduce the speed? How much more chip is removed per minute?

At constant T and ap: V2 · f20.4 = V1 · f10.4 → V2 = 200 · (0.25 / 0.35)0.4
(0,25 / 0,35)0,4 = 0,71430,4 = 0,8741 → V2 = 174.8 m/min
chip (Q = Vc · ap · f): 174,8 · 0,35200 · 0,25 = 61,1850 = 1,224
The feed rate is reduced to approximately 175 m/min, and 22% more chips are removed, with the same insert consumption

This is the rule in paragraph 26.12 explained in numerical terms: first, the greatest possible depth; second, the highest possible feed; and lastly, speed.

24.11 Minimum-Cost and Maximum-Output Speeds

Going faster shortens cutting time but wears out the cutting edges more quickly, and each change costs the price of the insert plus machine downtime. Going slowly saves on inserts but keeps the machine running longer. Between these two extremes, there is a speed that minimizes the cost per workpiece, and another, higher speed that minimizes the time per workpiece.

The cost per workpiece—for the portion that depends solely on speed—consists of three components: the cost of the machine while it is cutting, the cost of idle time (which does not change with speed), and the cost of the cutting edges, that is, the cost of the insert plus the changeover time. By applying Taylor’s law and seeking the minimum (with a bit of mathematical analysis), we arrive at two very simple formulas for the optimal cutting time:

Minimum Cost and Maximum Production Duration
Tc = (1n − 1) · (tcu + CuCm) Tp = (1n − 1) · tcu
Then the speeds using Taylor's method: Vc, minimum cost = CTc n Vc,max prod = CTp n
Tc Cutting edge life that results in the lowest cost, in minutes · Tp Duration at which maximum production is achieved, in minutes · n Taylor representative · twith Time required to change the cutting edge (machine downtime, resumption of adjustments), in min · Cu cost per cutting edge (price of the insert divided by the number of cutting edges, plus the tool holder dimension), in € · Cm Cost of the machine with an operator, in €/min

Formulas reveal interesting insights even without numbers. The maximum production time depends solely on the changeover time: when n = 0.25, it is 3 times tcu. The minimum-cost production time is always longer, so its rate is lower—the more expensive the inserts are relative to the machine, the lower the rate. Between these two speeds lies the optimal operating range, which some texts refer to as the “maximum efficiency range.”

Example 24.13 · Minimum-Cost and Maximum-Output Speeds

Carbide insert on C45: n = 0.25 and C = 430 m/min. The insert costs 12 € and has 4 cutting edges, so Cu = 3 € per cutting edge. Changing the cutting edge causes the machine to stop for 1.5 minutes. The machine with the operator costs 60 €/h, i.e., Cm = 1 €/min.

1/n − 1 = 1/0,25 − 1 = 4 − 1 = 3
Tc = 3 · (1.5 + 3 / 1) = 3 · 4.5 = 13.5 min
Vc,min cost = 430 / 13.50.25 = 430 / 1.9168 = 224.3 m/min
Tp = 3 × 1.5 = 4.5 min
Vc,max prod = 430 / 4.50.25 = 430 / 1.4565 = 295.2 m/min
Minimum cost at approximately 224 m/min (cutting edge lasts 13.5 min); maximum production at approximately 295 m/min (4.5 min)
Example 24.14 · Cost per Workpiece as Speed Varies

Using the same data, a workpiece requires 1.2 minutes of cutting time at 200 m/min (i.e., 240 meters of cutting: the cutting time is t = 240 / Vc) and has 1 minute of non-cutting time. The cost per workpiece is Cm · (downtime + t) plus the share of costs for cutting edges, (t / T) · (Cm · tcu + Cu) = (t / T) · 4.5 €.

at 200 m/min: t = 240 / 200 = 1.2 min; T = (430/200)⁴ = 21.37 min
machine: 1 · (1 + 1.2) = 2.200 €; cutting edges: (1.2 / 21.37) · 4.5 = 0.0562 · 4.5 = 0.253 €
Total at 200 m/min: 2.200 + 0.253 = 2.453 €
Vc (m/min)t (min)T (min)Car (€)Cutting edges (€)Cost (€)Time (min)
1501,60067,532,6000,1072,7072,636
2001,20021,372,2000,2532,4532,284
224,31,07013,512,0700,3562,4262,189
2500,9608,751,9600,4942,4542,125
295,20,8134,501,8130,8132,6262,084
3500,6862,281,6861,3543,0402,137
The minimum cost (€2.43) occurs precisely at 224 m/min, and the minimum time (2.08 min) occurs at 295 m/min

The time per workpiece in the last column is passive time + t + (t / T) · tcu. Notice how flat the curve is near the minimum: between 200 and 250 m/min, the cost changes by three cents. Beyond the maximum production speed, however, you lose out on both fronts: at 350 m/min, the workpiece costs more and takes longer to produce, because you spend all your time changing inserts.

1501802102402703003303600.511.522.533.50minimum €2.43Maximum production: 295minimum cost 224Total cost per workpiecemachine and operatortool and changesCutting speed Vc (m/min)cost per workpiece (€)
Figure 24.12 · The cost per workpiece from Example 24.14. The machine dimension (blue) decreases with speed, while the cutting edge dimension (green) increases at an ever-faster rate; the total cost (red) has a broad, flat minimum.
💡
When maximum production is most cost-effective. If the machine is the department’s bottleneck, every minute saved is worth more than the cost of the insert: in that case, you should aim for the maximum production speed. If, on the other hand, the machine has idle time, it’s best to stay close to the minimum cost. The complete calculation of the cost of a workpiece, including all processing times, is provided in Chapter 30.

24.12 Coolant-lubricants

The cutting fluid has three functions: to cool the tool and the workpiece, to lubricate the contact between the chip, the rake face, and the flank, and to remove the chip from the cutting zone. In addition, it must protect the workpiece and the machine from rust, ensure the safety of the operators, and not spoil in the tank.

  • Emulsions (“white water”): emulsifiable oil dispersed in water, typically at a concentration of 3–8%. Water cools very effectively, while oil provides some lubrication and protects against rust. These are the most commonly used fluids for turning and milling. The following parameters must be monitored: concentration, pH, bacteria, and any foreign oil floating on the surface.
  • Full-film oils (pure cutting oils, often containing high-pressure additives): They provide high lubrication but little cooling. They are used where friction is more important than heat: tapping, threading, broaching, gear cutting, automatic lathes, and profile grinding. Fumes and fire hazards require enclosed, vented machines.
  • Synthetic and semi-synthetic fluids: clear solutions containing little or no mineral oil; they provide excellent cooling, are clean, and are widely used in grinding.
  • Minimal (MQL): a few dozen milliliters of oil per hour, atomized with compressed air directly onto the cutting edge. Lubricates without cooling; the chips come out almost dry and are recyclable. Excellent for aluminum, deep drilling with suitable tools, and automated production lines.
  • Dry cutting: no coolant. With coated carbide, ceramic, and CBN, this is often the best choice for steels and cast iron, especially in milling: intermittent coolant flow causes thermal cracks (section 24.8). Good chip evacuation is required, often using air.
  • High pressure (70 bar and above, through the tool): the jet enters between the chip and the tool face, cools the hottest area, lifts the chip, and breaks it off. This is the solution for stainless steel, titanium, and superalloys, as well as for deep drilling.
Machining operations or materialA typical choice
Turning and milling of steel using HSSa generous amount of emulsion
Turning of Steel with Carbideemulsion, or dry
Milling of steel and cast iron with carbidedry or air; if using fluid, use it generously and continuously
gray cast irondry (graphite acts as a lubricant; powder mixed with emulsion creates sludge)
aluminumemulsion or MQL
stainless steel, titanium, superalloyshigh-pressure emulsion
tapping, threading, broachingwhole oil or highly concentrated emulsion
correctionemulsion or synthetic; full-oil for profiles and tools

General guidelines: The tool supplier and the fluid supplier provide recommendations for specific cases.

Example 24.15 · Preparing and Checking the Emulsion

The tank of a lathe holds 400 liters, and the supplier recommends a 5% emulsion. How much oil is needed? After one week, the refractometer reads 3.2, and the oil correction factor, listed on the technical data sheet, is 1.5. What is the concentration of the emulsion?

oil = 400 × 0.05 = 20 liters, and 380 liters of water
concentration = reading × factor = 3.2 × 1.5 = 4.8%
20 liters of oil; after a week, the level is at 4.8%, still within the specified range

Workshop rule: Pour oil into water, never water into oil; otherwise, the emulsion “goes haywire” and separates. An emulsion that’s too thin causes rust and wears down tools; one that’s too thick foams, irritates the skin, and is costly.

⚠️
Health and the Environment. Cutting fluids must be handled with appropriate gloves and kept away from open wounds; mist must be extracted. Spent emulsions are classified as special waste and must be disposed of through authorized companies—never down the drain.

24.13 Machinability of Materials

The machinability (or machinability) indicates how easy it is to remove chips from a material: how long the tool lasts, what forces are required, what kind of chips are formed, and what kind of surface is obtained. In section 20.12, we discussed this in relation to theworkability index of steels, relative to free-cutting steel 11SMn30 = 100. Taylor’s law explains where this number comes from: it is the ratio of the speeds that yield the same duration of the cutting edge on the two materials, using the same tool.

Relative Machinability
I2I1 = VT,2VT,1
I1, I2: workability indices of the two materials · VT,1, VT,2: cutting speeds that result in the same tool life T (for example, 15 minutes) for the two materials, in m/min
Example 24.16 · Stainless steel vs. C45, using the same insert

With the same carbide insert, endurance tests show n = 0.25 and C = 430 m/min for normalized C45, and n = 0.22 and C = 318 m/min for 304 stainless steel. What feed rates result in a 15-minute service life? What is the index for 304, if C45 has an index of 40?

C45: V15 = 430 / 150.25 = 430 / 1.9680 = 218.5 m/min
304: V15 = 318 / 150.22 = 318 / 1.8144 = 175.3 m/min
ratio = 175.3 / 218.5 = 0.802 → index of 304 = 40 · 0.802 = 32.1
The 304 maintains about 80% of the C45's speed: index 32, as shown in Figure 20.9

ISO Material Groups

To select the right tool, the materials to be machined are divided into six ISO groups, each identified by a letter and a color that appear in all insert catalogs. Within a group, the cutting challenges are similar; the appropriate insert grade for each group is discussed in Chapter 25.

GroupMaterialsHow do they perform when cutting?
P · blueunalloyed and alloyed steels, cast steels, ferritic and martensitic stainless steelsLong, continuous chips that need to be broken up; flank wear and cratering
M · yellowaustenitic and duplex stainless steelsSticky, become hardened, poor heat conductivity: cutting edge, nicks, heat at the tip
K · redgray cast iron, spheroidal cast iron, malleable cast ironshort chips; abrasive wear; dust
N · greenaluminum, copper, brass, bronze, plasticsLow force, high speed; tendency to stick: sharp, polished cutting edge
S · orangenickel-cobalt superalloys, titaniumheat-resistant, segmented chips, heat on the cutting edge: low speeds
H · grayhardened steels (over approximately 45 HRC), hard cast ironHigh forces, segmented chips; CBN and ceramic, negative rake angle

We saw in Chapter 20 what makes a material difficult to machine: high hardness (or, conversely, a material so soft that it becomes dough-like), toughness and work hardening, hard carbides, and low thermal conductivity. The sulfur and lead inclusions in free-cutting steels and turning brasses improve machinability by breaking up the chips and providing lubrication.

24.14 Chip Control

A strip of hot steel chips, a few meters long, wraps itself around the workpiece and the spindle, scrapes the freshly machined surface, breaks the inserts, and can injure whoever removes it. On an automatic machine, a tangle of chips can block the loader or conveyor. The chips must therefore be broken into short workpieces: the best shapes are short spirals, “commas,” and curls shaped like a 6 or a 9.

The chip breaks if it is bent enough to snap on its own. This bending is achieved by the chip breaker: a feature machined into the face of the insert (a groove, ridges, or a step), or a small plate attached to brazed tools. As the chip exits, it strikes the chip breaker, bends sharply, and breaks upon hitting the workpiece or the tool. Each geometry works well only within a certain range of feeds and cutting depths, which the supplier draws in an f-ap diagram (Figure 24.13):

short chip,well-brokenchip breaker arealong, ribbon-like chipsor tangledcoarse pass, small f:long spiralschips too compressed:overloaded insertlarge f, small pass:hard chips, vibrationsfeed rate f (mm/rev)cutting depth ap (mm)
Figure 24.13 · Qualitative diagram of a chipbreaker’s working area. Each insert geometry has its own: finishing geometries are at the bottom left, roughing geometries at the top right.
  • Feed rate too low: The chip is thin and flexible; it bends without breaking and forms a ribbon. The first solution is almost always to increase the feed rate;
  • The depth is too small relative to the nose radius: only the tip arc is engaged, and the chip does not reach the chip breaker;
  • Excessive feeds and depth of cut: The chip is thick, hard, and too tightly compressed; the insert is overloaded and at risk of breaking;
  • If you can't change the parameters, change the geometry: finishing geometries have a narrow chipbreaker close to the cutting edge, while roughing geometries have a wide, robust chipbreaker. A smaller κr value, which produces thinner chips, or high-pressure coolant can also help.

Vibrations and Chatter

When the tool or workpiece vibrates, regular lines appear on the surface, the machine “sings,” and the cutting edges chip. The most troublesome type of vibration is self-excited vibration, known as chatter: the cutting edge vibrates and leaves a wavy surface; on the next pass, it encounters a varying chip thickness, which in turn causes the cutting force to vary and feeds the vibration. All it takes is exceeding a certain depth of cut for the phenomenon to start and grow on its own.

Chatter is primarily countered by rigidity. The deflection of an overhanging tool increases with the cube of the stick-out (Section 10.10 and Examples 10.15 and 10.16), therefore:

  • Keep tools, boring bars, and workpieces protruding as little as possible; for boring bars, the rule of thumb is approximately 4 times the diameter for steel, 6 times for carbide, and more than 10 times for anti-vibration bars;
  • Choose the largest tool holder and bar that will fit; use the tailstock or chuck for long workpieces;
  • reduce the radial force: κr close to 90°, small nose radius, positive rake angle, and sharp cutting edge;
  • Adjust the cutting speed (often by as little as 10–20%) to move away from the critical frequency; sometimes it is better to increase the feed rate rather than decrease it, because a chip that is too thin causes the cutting edge to skid.
Example 24.17 · Thicker or Shorter Bar?

The stiffness of a cantilever beam, for a given material, is proportional to d⁴ / L³ (from the deflection formula, where I = π · d⁴ / 64). A hole is drilled with a Ø20 bar that protrudes 100 mm. How much stiffness is gained by switching to a Ø25 bar with the same stick-out? And how much stiffness is lost by keeping the Ø20 bar but extending it to protrude 150 mm?

Ø25 vs. Ø20, same L: (25 / 20)⁴ = 1.254 = 2.441
Ø20, from 100 to 150 mm: stiffness × (100 / 150)³ = 1 / 1.53 = 1 / 3.375 = 0.296
The Ø25 bar is 2.4 times stiffer; stretching the Ø20 bar by 50% makes it 3.4 times more flexible
🖥️
Try it in CNC Code. In the lathe simulator, try machining the same workpiece with different speeds and feeds: the varying machining time, shown in the table in Example 24.14, will let you see for yourself where the minimum-cost speed lies.

24.15 The Formulas in This Chapter

What Are You Looking For?FormulaUnits
Tracing Ratioλ = h′ / hpure number
Chip Speed at the FaceVtr = Vc / λm/min
Sliding angletan φ = cos γ / (λ − sin γ)degrees
Cross-Sectional Anglesα + β + γ = 90°degrees
Angles in a floor planκr + εr + κr′ = 180°degrees
Forward and passive forceFf = Fn · sin κr · Fp = Fn · cos κrN
Correction of kc for γkc,γ ≈ kc · (1 − (γ − γ0) / 100)N/mm²
Average chip temperatureΔT ≈ ηtr · kc / (ρ · c)°C
Taylor's LawVc · Tn = C · T = (C / Vc)1/nm/min, min
A representative from two roundsn = log (V1 / V2) / log (T2 / T1)pure number
Extended TaylorVc · Tn · fa · apb = C1m/min
Minimum Cost DurationTc = (1/n − 1) · (tcu + Cu / Cm)min
Maximum Production DurationTp = (1/n − 1) · tcumin
Cost per workpiece (variable portion)Cm · (t0 + t) + (t / T) · (Cm · tcu + Cu)€
Relative MachinabilityI2 / I1 = VT,2 / VT,1pure number

Cutting speed, force, specific pressure, and turning power are listed in Table 26.14.

24.16 Exercises

Try to solve them on your own, using a calculator, before looking at the solution.

Exercise 1. A tool has α = 8° and γ = −5°. What is the value of the cutting angle β?
Solution

β = 90° − 8° − (−5°) = 90° − 8° + 5° = 87°.

Exercise 2. A 55° rhomboidal insert is mounted on a tool holder with κr = 93°. What are the values of the point angle and the secondary clearance angle?
Solution

εr = 55° (this is the shape of the insert); κr′ = 180° − 93° − 55° = 32°.

Exercise 3. In a perpendicular cut, the cut layer is 0.2 mm thick and the chip is 0.5 mm thick; γ = 10° and Vc = 150 m/min. Find λ, φ, and the chip speed.
Solution

λ = 0.5 / 0.2 = 2.5. tan φ = cos 10° / (2.5 − sin 10°) = 0.9848 / (2.5 − 0.1736) = 0.9848 / 2.3264 = 0.4233, φ = 22.9°. Vtr = 150 / 2.5 = 60 m/min.

Exercise 4. When n = 0.25, a cutting insert lasts 20 minutes at 200 m/min. How long does it last at 160 m/min?
Solution

T2 = T1 · (V1 / V2)¹/n = 20 · (200 / 160)⁴ = 20 · 1.254 = 20 · 2.4414 = 48.8 min. Or: C = 200 · 200.25 = 422.9 and T = (422.9 / 160)⁴ = 48.8 min.

Exercise 5. Two endurance tests yield the following results: 150 m/min → 60 minutes, 225 m/min → 12 minutes. Find n and C.
Solution

n = log (225 / 150) / log (60 / 12) = log 1.5 / log 5 = 0.17609 / 0.69897 = 0.2519. C = 150 · 600.2519 = 150 · 2.8052 = 420.8 m/min (check: 225 · 120.2519 = 420.8).

Exercise 6. The cutting speed is increased by 10%. By how much does the cutting edge life decrease for an HSS tool (n = 0.125), a carbide tool (n = 0.25), and a ceramic tool (n = 0.5)?
Solution

T2 / T1 = 1.1−1/n. HSS: 1.1−8 = 0.467; service life decreases by 53%. Carbide: 1.1−4 = 0.683, tool life decreases by 32%. Ceramic: 1.1−2 = 0.826, tool life decreases by 17%.

Exercise 7. An insert with n = 0.25 and C = 400 m/min costs €5 per cutting edge; changing the insert takes 2 minutes, and the machine costs €72 per hour. Find the minimum-cost and maximum-output speeds.
Solution

Cm = 72 / 60 = 1.2 €/min. Tc = 3 · (2 + 5 / 1.2) = 3 · 6.1667 = 18.5 min, V = 400 / 18.50.25 = 400 / 2.0739 = 192.9 m/min. Tp = 3 × 2 = 6 min, V = 400 / 60.25 = 400 / 1.5651 = 255.6 m/min.

Exercise 8. A batch of 1,200 workpieces requires 0.9 minutes of cutting time per workpiece. Each cutting edge lasts 15 minutes, and each insert has 6 cutting edges. How many inserts are needed?
Solution

Number of cutting edges = 15 / 0.9 = 16.67 → 16 (rounded down). Cutting edges = 1200 / 16 = 75. Inserts = 75 / 6 = 12.5 → 13 inserts.

Exercise 9. An aluminum alloy is being cut with kc = 700 N/mm². Given ρ = 2.7 g/cm³, c = 0.9 J/(g·K), and 80% of the heat is absorbed by the chip, by how much does the chip heat up on average?
Solution

ρ · c = 2.7 · 0.9 = 2.43 J/(cm³·K). ΔT ≈ 0.8 × 700 / 2.43 = 230 °C. This is much less than in steel (Example 24.7): aluminum requires very little energy per cm³.

Exercise 10. After 1.5 minutes of running-in, flank wear is VB = 0.05 mm; it then increases by 0.02 mm per minute. After how much cutting time does VB reach 0.3 mm? And what about when the finishing criterion is VB = 0.2 mm?
Solution

VB 0.3: T = 1.5 + (0.3 − 0.05) / 0.02 = 1.5 + 12.5 = 14 min. VB 0.2: T = 1.5 + (0.2 − 0.05) / 0.02 = 1.5 + 7.5 = 9 min.

Exercise 11. A boring bar protrudes by 4 times its diameter. To reach the bottom of a hole, it must protrude by 6 times its diameter. By how much does the deflection increase under the same force?
Solution

The deflection is proportional to L³: (6 / 4)³ = 1.53 = 3.375. The deflection becomes about 3.4 times greater: it is advisable to switch to a hard metal or vibration-damping bar.

Exercise 12. Machining is performed at 160 m/min with f = 0.3 mm/rev. To improve roughness, the feed rate is reduced to f = 0.2 mm/rev. Using the extended Taylor’s law and a = 0.4, to what speed can the feed rate be increased while maintaining the same tool life? Does the chip volume per minute increase or decrease?
Solution

V2 = 160 · (0.3 / 0.2)⁰.⁴ = 160 · 1.5⁰.⁴ = 160 · 1.1761 = 188.2 m/min. Volume ratio: (188.2 × 0.2) / (160 × 0.3) = 37.64 / 48 = 0.784: the chip removal rate per minute decreases by approximately 22%.

Exercise 13. For an alloy steel, the specific pressure calculated using the data in the table (valid for γ0 = 6°) is 2200 N/mm². What value is estimated using an insert with a positive correction factor for γ = 18°?
Solution

kc,γ ≈ 2200 · (1 − (18 − 6) / 100) = 2200 · 0.88 = 1936 N/mm².

Exercise 14. A cutting operation absorbs Pc = 4 kW. With 75% of the heat in the chips, 15% in the tool, and 10% in the workpiece, how much thermal power does each receive?
Solution

Chip 0.75 × 4 = 3 kW; tool 0.15 × 4 = 0.6 kW; workpiece 0.10 × 4 = 0.4 kW.