Steel is the most commonly used material in the workshop, but it isn't always the best choice. When a workpiece needs to be lightweight, conduct electricity or heat, resist rust, slide without lubricant, or be machined quickly on an automatic lathe, aluminum, copper and its alloys, titanium, and plastics come into play. In this chapter, we’ll learn how to identify them by their designations, understand what each material can be used for, and how they behave under the tool, along with the calculations needed to make the right choice.

21.1 Nonferrous Metals: Why We Need Them and How Much They Weigh

Non-ferrous metals are all metals and alloys in which iron is not the main element: aluminum, copper, zinc, titanium, magnesium, nickel, tin, lead, and their alloys. Almost all of them cost more than steel on a weight-for-weight basis, so they are chosen when they offer something that steel does not:

  • lightweight: aluminum, magnesium, and titanium weigh between one-quarter and just over half as much as steel;
  • electrical and thermal conductivity: copper and aluminum for cables, busbars, heat exchangers, and heat sinks;
  • corrosion resistance without coating: aluminum, copper, bronzes, titanium;
  • machinability: brass for turning and some aluminum alloys can be cut much more quickly than steel;
  • ease of casting: zinc and aluminum are cast into steel molds at low temperatures;
  • Special properties: low friction of bronzes and white metals, biocompatibility of titanium, heat resistance of nickel superalloys.

The first quantity to compare is the density ρ, which we learned about in Chapter 2. The figure files the materials covered in this chapter; the dashed line represents steel.

PE-UHMW0.93PA61.14POM1.41magnesium1.74PTFE2.2aluminum2.7titanium4.5Zama (zinc)6.7steel7.85brass8.5bronze8.8copper8.9nickel8.9lead11.3WC-Co cemented carbide14.5plasticsnon-ferrous metalssteel
Figure 21.1 · Approximate densities in kg/dm³. Engineering plastics range from 0.9 to 2.2; titanium falls halfway between aluminum and steel; copper and its alloys are heavier than steel.
Mass of a workpiece
m = ρ · V m2m1 = ρ2ρ1
m mass in kg · ρ density in kg/dm³ · V volume in dm³ (1 dm³ = 1,000,000 mm³). For objects of the same shape, the ratio of their masses is equal to the ratio of their densities.
Example 21.1 · The Same Flange in Three Metals

A flange is a 120-mm-diameter disc that is 20 mm thick, with a 40-mm-diameter hole in the center. How much does it weigh when made of steel, aluminum, and titanium?

V = π/4 · (120² − 40²) · 20 = 0.7854 · (14,400 − 1,600) · 20 = 0.7854 · 12,800 · 20 = 201,062 mm³ = 0.20106 dm³
steel: m = 7.85 × 0.20106 = 1.578 kg
aluminum: m = 2.7 × 0.20106 = 0.543 kg
titanium: m = 4.5 × 0.20106 = 0.905 kg
ratios: 2.7 / 7.85 = 0.344 and 4.5 / 7.85 = 0.573
1.58 kg of steel, 0.54 kg of aluminum (about one-third), 0.90 kg of titanium (just over half)

21.2 Aluminum

Where does it come from?

Aluminum is the most abundant metal in the Earth's crust, but it is never found in its pure form in nature: it is bound to oxygen. The mineral from which it is extracted is the bauxite. In the first step, the bauxite is dissolved in caustic soda, and thealumina (aluminum oxide, Al2O3), a white powder. In a second step, the alumina is melted in a bath of molten salts at about 950 °C, and the metal is separated using an electric current (electrolysis). Roughly speaking, it takes 4 metric tons of bauxite to produce 2 metric tons of alumina, and 2 metric tons of alumina to produce 1 metric ton of aluminum, with very high electricity consumption. That is why the recycling It's so important: Remelting chips and scrap costs only a small fraction of the energy required to produce the metal from ore. In the workshop, aluminum chips are kept separate from steel chips precisely because they're worth more.

The Properties

  • Lightweight: ρ = 2.7 kg/dm³, about one-third that of steel. The alloys range from 2.65 to 2.8 kg/dm³.
  • Low module of elasticity: E ≈ 70,000 N/mm², one-third that of steel. For the same shape and load, a workpiece of aluminum deflects three times as much, even if the alloy is strong (Chapter 10).
  • It melts at 660 °C (pure aluminum; alloys melt a little earlier) and does not change color when heated: welding it requires experience.
  • He drives well Electricity and heat: Copper offers about 60% of the electrical conductivity of other materials, with less than one-third of their mass.
  • It expands a lot: α ≈ 23 · 10−6 /°C, twice that of steel. Take this into account when taking measurements and when making fits for workpieces made of steel.
  • It is corrosion-resistant because, when exposed to air, it immediately forms a very thin layer of oxide—hard and tightly adherent—that protects the metal beneath. This layer breaks down in highly acidic or highly alkaline environments and in the presence of chlorides (seawater), where some alloys are susceptible to corrosion.

Anodizing

Anodizing (or anodic oxidation) artificially thickens the oxide layer. The workpiece is immersed in an acid bath and connected to the positive terminal (the anode) of a power source: the current causes a porous oxide layer to form, which is then sealed in hot water. Before sealing, the pores can be filled with dye: this is how black, red, or blue workpieces are made. There are two types:

  • standard anodizing (protective and decorative), 5 to 25 μm: protects against corrosion and provides color;
  • Hard anodizing (thick-film), approximately 25 to 75 μm thick, performed at low temperatures: it produces an extremely hard, wear-resistant, and electrically insulating surface.

The oxide does not settle on the surface of the workpiece like paint: it forms by transforming the metal itself. For this reason, part of the oxide layer grows outward, and part penetrates into the workpiece. In standard anodizing, about one-third of the layer grows outward, while in hard anodizing, about half does. For precision workpieces, this must be taken into account during the machining process.

aluminum porous Al₂O₃ oxide, then sealed toward the outside: from 1/3 to 1/2 inside the metal: the remainder surface before the bath
Figure 21.2 · Cross-section of an anodized surface, with thicknesses greatly magnified. The red line represents the surface of the workpiece before anodizing: the oxide layer lies partly on top and partly underneath.
Example 21.2 · A pin to be anodized to a specific thickness

A 6082 alloy pin must measure Ø40.000 mm after a 50 μm hard anodizing process. Half of the thickness increases toward the outside. To what diameter should it be turned?

increase in radius = 50 / 2 = 25 μm = 0.025 mm
Increase in diameter = 2 × 0.025 = 0.050 mm
turning diameter = 40.000 − 0.050 = 39.950 mm
It is turned to Ø39.950: without this adjustment, the pin would come out at Ø40.050
🔩
Holes, threads, and edges. In holes, the oxide layer grows toward the center, so the diameter decreases; tight threads can become clogged and must be protected with plugs or reworked afterward. Oxide breaks down on sharp edges: the parts to be anodized should be designed with small radii or chamfers.

21.3 Aluminum Alloys

Pure aluminum is soft: its tensile strength is approximately 100 N/mm². By adding small amounts of other elements (copper, magnesium, silicon, zinc, manganese), alloys can be produced with tensile strengths of 550 N/mm² and higher. Alloys are divided into two main categories: those for plastic machining operations, which are supplied as bars, sheets, plates, tubes, and profiles produced by rolling, extrusion, or drawing; and those for foundry use, which are cast into shapes.

Alloys for machining operations: the EN AW designation

According to European standards, the designation is EN AW-6082: A stands for aluminum, and W stands for “wrought,” meaning it has been plastically worked. The four digits are interpreted as follows:

  • The first digit indicates the main alloying element, and thus the series;
  • The second digit indicates a variant of the original alloy (0 is the base alloy);
  • The last two digits identify the alloy within the series (in the 1000 series, they indicate the purity: 1050 means at least 99.50% aluminum).

Next to the number, you’ll find the chemical formula in square brackets, which lists the elements: EN AW-6082 [AlSi1MgMn] contains about 1% silicon, plus magnesium and manganese. In the workshop and on suppliers’ price lists, it is simply referred to as “6082,” or old trade names are still used, such as Anticorodal for the 6000 series, Avional for the 2000 series, and Ergal for 7075.

SeriesMain ElementHeat-treatableFeaturesAlloys and Typical Applications
1000at least 99% aluminumnosoft, conductive, corrosion-resistant1050: sheet metal, conductors, heat exchangers, packaging
2000copperyesdurable, not very resistant to corrosion2011: automatic turning (short chips); 2024: aerospace; 2014: stamped workpieces
3000manganesenomedium strength, excellent formability3003: cans, covers, heat exchangers
4000siliconUsually notIt sinks lower, flows well4043: welding wire
5000magnesiumnoExcellent corrosion resistance, including in marine environments; weldable5083: plates, hulls, tanks; 5754: bent sheet metal, car bodies
6000magnesium and siliconyesA good compromise; it extrudes and anodizes well6060: profiles for windows and doors; 6082: bars and plates for mechanical applications; 6061
7000zinc (with magnesium and copper)yesthe most durable, difficult to weld7075: molds, tooling, aerospace, sports
8000other elements (iron, lithium)It dependsspecial alloys8011: thin sheets; lithium alloys for aircraft

The following table lists the mechanical properties of some alloys commonly used in workshops. For 6082 and 7075, the values are the same as those in Table 10.4.

The League and the StateRe (N/mm²)Rm (N/mm²)A%Machinability
EN AW-1050A H14851106Poor: clumpy, long chips
EN AW-2011 T327033010Excellent: short chips, designed for automatic lathes
EN AW-5083 H11113028015moderate: tender, tends to become doughy
EN AW-6060 T61602008moderate
EN AW-6082 T626031010Good, long chips that are hard to break
EN AW-7075 T6 / T6514805508Excellent: hard, very smooth surfaces

These are approximate, average, and rounded values compiled by us. They vary depending on the thickness and shape of the semi-finished product; for projects, use the minimum values guaranteed by the product standard or certificate.

Delivery Conditions

After the alloy number comes the heat treatment designation, separated by a hyphen: this indicates what was done to the metal after production, and it can even double the strength. A 6082 bar in the O (annealed) condition and one in the T6 condition are made of the same alloy, but the latter is more than twice as strong.

Alloys in the 1000, 3000, and 5000 series do not harden when heated: they are strengthened only by cold working (rolling, drawing), through work hardening, and their condition is indicated by the letter H. Alloys in the 2000, 6000, and 7000 series require heat treatment: they harden through a cycle of solution treatment, quenching, and aging, and their condition is indicated by the letter T.

StatusMeaningWhere is it located?
Fblank, no property testingNon-warrantied semi-finished products
Oannealed: the softest and most ductilesheet metal for deep drawing, workpieces requiring heavy bending
H111annealed with slight work hardening due to flattening5083 and 5754 plates and sheets
H12, H14, H16, H18work-hardened to 1/4, 1/2, 3/4, and fully hardenedsheets from the 1000 and 3000 series
H22, H24work-hardened and then partially annealed: slightly more ductile while maintaining the same strengthsheets of metal to be bent
H32, H34work-hardened and stabilized at low temperature5000 series alloys
T3solution-treated, cold-formed, naturally aged2011, 2024
T4dissolved and aged naturally at room temperatureworkpieces to be formed after treatment
T5cooled upon exiting the extruder and artificially aged6060 extrusions
T6solution-treated, quenched, and artificially aged: maximum strength6082, 6061, 7075
T651T6 plus stress relief annealing: the plate is stretched by a few thousandths to relieve the stresses from the hardening processplates and bars for milling
T73overaged: slightly less durable, much less susceptible to stress corrosion7075 for the aerospace industry
20170530°Csolubilizationsolubilization, approximately 530 °Cquenchingin waterT6: artificial agingapproximately 170 °C for 8–10 hoursT4: natural aging, several days at room temperature
Figure 21.3 · Typical thermal cycle of a 6082 alloy. Solution treatment dissolves the alloying elements into the aluminum; quenching “freezes” them in their dissolved state; and aging causes them to precipitate as extremely fine particles that harden the metal.
🧱
Why is T651 specified for milling? After heat treatment, a plate has high internal stresses: the surface cools faster than the core. If a large amount of material is removed from just one side, the stresses are released and the workpiece warps as soon as it is released from the vise. Stretching the T651 material removes most of these stresses: for molds, tooling plates, and hollow workpieces, 7075-T651 or 6082-T651 is always ordered.

Foundry Alloys: The EN AC Designation

Cast alloys are designated with EN AC (where “C” stands for “cast”) followed by five digits, often followed by the chemical symbol: for example, EN AC-46000 [AlSi9Cu3(Fe)]. Here, too, the first digit indicates the main element: 2 for copper, 4 for silicon, 5 for magnesium, 7 for zinc. Almost all casting alloys contain silicon, because silicon lowers the melting temperature and makes the alloy very fluid: it fills thin molds well and shrinks very little as it solidifies. The alloy with about 12% silicon (AlSi12) has the lowest melting point, around 577 °C.

  • EN AC-46000 [AlSi9Cu3(Fe)]: the most common alloy for die casting (casings, housings, brackets); the iron in parentheses indicates that a slightly higher amount is allowed, as it helps prevent sticking to the mold.
  • EN AC-42100 [AlSi7Mg0.3]: sand-cast and shell-cast workpieces to be heat-treated (T6), for wheels, suspension components, and structural workpieces.
  • EN AC-44100 [AlSi12(b)]: thin-walled castings, excellent fluidity, excellent corrosion resistance.
  • Hypereutectic alloys (containing more than 12% silicon, such as AlSi17Cu4): wear-resistant pistons and cylinders.

Silicon is hard and abrasive: the more silicon there is, the faster the tool wears out. For alloys with a high silicon content, fine-grain carbide or polycrystalline diamond (PCD) inserts are used (see Chapter 25).

Example 21.3 · Reading Abbreviations

What do these abbreviations mean—the ones you find on drawings and delivery slips?

EN AW-6082-T6: alloy for machining operations, 6000 series (magnesium and silicon), solution-treated and artificially aged; Rm approximately 310 N/mm²
EN AW-2011-T3: 2000 series (copper), free-cutting alloy, solution-treated, cold-drawn, and naturally aged
EN AW-5083-H111: 5000 series (magnesium), not heat-treatable, annealed and freshly rolled; suitable for marine environments
EN AW-7075-T651: 7000 series (zinc), T6 temper with stress relief by stretching; the right plate for a milling die
EN AC-46000 [AlSi9Cu3(Fe)]: a foundry alloy containing silicon (approximately 9%) and copper (approximately 3%), for die casting
Letter W = machining operations, C = foundry; first digit = alloy element; the status follows the hyphen

21.4 Aluminum in Machine Tools

Aluminum alloys are among the easiest materials to cut: the cutting force is about one-third that of steel, and the heat is dissipated through the chips and into the workpiece, which is a good heat conductor. This allows for very high cutting speeds, ranging from 300 to 1,500 m/min with carbide (Table 26.12), which are usually limited by the spindle speed rather than by the tool itself. The real problems are twofold: long chips and the built-up cutting edge.

tool chip material to be removed cutting edge aluminum welded to the cutting edge aluminum alloy workpiece the workpiece moves against the tool at a speed of Vc
Figure 21.4 · The built-up cutting edge: aluminum particles weld onto the tip, alter the geometry of the cutting edge, and then break off, carrying away fragments of the insert and scratching the surface.

A built-up edge forms when hot aluminum under pressure fuses to the cutting edge. Here's how to prevent it:

  • Inserts specifically designed for aluminum (ISO N group): very sharp cutting edge, large and positive top rake angle, mirror-polished face, usually uncoated or with smooth coatings such as DLC (diamond-like carbon); Standard coatings for steel are rough, and aluminum tends to stick to them;
  • high speed: at low speeds, more material builds up;
  • plenty of coolant or minimum (MQL), which reduces friction on the chest;
  • Two- or three-flute cutters with wide grooves, because the chips are large, and if they get stuck in the groove, they will clog it and break the tool.

Soft alloys (1050, 5083 ricotta) produce more chips; hard alloys (7075-T6, 2011-T3) cut better and produce smoother surfaces. 6082-T6 produces long chips: when turning, you’ll need inserts with chip breakers for aluminum and feeds that aren’t too low.

Example 21.4 · High RPMs for Aluminum

A 6082 bar with a diameter of 40 mm is turned at Vc = 500 m/min, then a pocket is milled using a 16 mm end mill at Vc = 600 m/min. The milling machine’s spindle reaches 10,000 rpm.

lathe: n = 1000 · 5003,1416 · 40 = 3978.9 rpm → S3980
cutter: n = 1000 · 6003,1416 · 16 = 11,936.6 rpm: above the limit
at maximum speed: Vc = 3.1416 × 16 × 10,000 / 1,000 = 502.7 m/min
Lathe at 3,980 rpm; the milling cutter operates at 10,000 rpm and approximately 500 m/min, because it controls the spindle
Example 21.5 · Measuring Aluminum While It's Still Hot

A 200-mm-long workpiece of aluminum comes out of the machine at 32 °C and is measured immediately. How much will it shrink when it returns to 20 °C? What if it were made of steel?

ΔT = 32 − 20 = 12 °C
aluminum: ΔL = α · L · ΔT = 23 · 10−6 · 200 · 12 = 0.0552 mm
steel: ΔL = 11.5 × 10−6 · 200 · 12 = 0.0276 mm
More than 5 cents for aluminum, twice as much as steel: tight dimensions are checked on cold workpieces

21.5 Copper and Its Alloys

Copper

Copper (Cu) is extracted from ores containing copper sulfides: the ore is concentrated, smelted, refined, and finally purified by electrolysis to 99.9% purity. It has a density of 8.9 kg/dm³ and melts at 1085 °C. Its most important property is electrical conductivity, the best among base metals after silver: this is why copper is used in cables, motor windings, and busbars in electrical panels. It is also an excellent heat conductor (heat exchangers, welding machines, spot-welding electrodes) and is highly resistant to corrosion: when exposed to air, it develops a green patina that protects it.

Copper for electrical applications is called Cu-ETP (99.9%, with a small amount of oxygen); Cu-OF is oxygen-free and welds and solders better. Pure copper is “sticky” when machined: it clings to the cutting edge and causes burrs. Very sharp, high-quality tools are needed, just as with aluminum. Electrodes for electrical discharge machining are often made of copper or graphite.

MaterialElectrical conductivity σ (MS/m)% copper (IACS)Thermal conductivity (W/(m·K))
Copper Cu-ETP58100390
Pure aluminum for conductors3560230
Alloy 6082-T62543170
Brass CuZn39Pb31526120
Non-alloy steel61050
Austenitic stainless steel1,42,415
Titanium Ti6Al4V0,617

Approximate values at 20 °C, rounded. IACS is the international scale that assigns a value of 100 to annealed copper as the reference.

Electrical Resistance of a Conductor
R = Lσ · A
R resistance in Ω · L length in m · σ conductivity in MS/m (megasiemens per meter) · A cross-sectional area in mm². With these units, the powers of ten cancel each other out, and R is directly expressed in ohms.
Example 21.6 · Copper or Aluminum for a Long Line

A wire is 100 m long and has a 10 mm² copper conductor. What cross-sectional area must an aluminum conductor have to have the same resistance, and how much do the two conductors weigh?

copper: R = 100 / (58 × 10) = 0.1724 Ω
The same R value for aluminum: A = 10 · 58 / 35 = 16.57 mm² (check: 100 / (35 · 16.57) = 0.1724 Ω)
Volume of copper: 10 mm² · 100,000 mm = 1,000,000 mm³ = 1 dm³ → m = 8.9 · 1 = 8.90 kg
Volume of aluminum: 16.57 × 100,000 = 1,657,000 mm³ = 1.657 dm³ → m = 2.7 × 1.657 = 4.47 kg
Aluminum requires a cross-section that is 66% larger but weighs about half as much; that is why high-voltage power lines are made of aluminum

Brass Instruments

Brass is an alloy of copper and zinc (CuZn), containing approximately 5% to 45% zinc. More zinc means greater strength and lower cost, up to a certain point:

  • Up to about 37% zinc, brass has a single phase (α) and is very flexible cold: it is deep-drawn, bent, and drawn (CuZn37, brass for sheet metal and tubing; CuZn30 for casings and heat exchanger tubes);
  • Above 37%, a second, harder phase (β) appears: α + β brass is easy to work with when hot (for pressing fillets and valves) and cuts more easily.

The European designation is either symbolic—with chemical symbols followed by percentages (CuZn39Pb3: copper and the remainder, approximately 39% zinc and 3% lead)—or numerical, such as CW614N. In the numerical designation, the first letter C stands for copper, the second for the product type (W for plastic machining, C for castings, B for ingots), followed by three digits and a final letter indicating the group: for example, L and M for brass alloys consisting only of copper and zinc, N and P for leaded brass, and R and S for special brass alloys.

CuZn39Pb3 (CW614N) turning brass is the benchmark material for machinability: the lead, which does not dissolve in the alloy, remains in scattered droplets that break the chip into fine flakes. On automatic lathes, machining is performed at high speeds with very short chips, producing smooth surfaces and ensuring extremely long tool life. Re ≈ 250 N/mm², Rm ≈ 430 N/mm² (Table 10.4). For workpieces that come into contact with drinking water, regulations are increasingly restricting the use of lead: low-lead or lead-free brasses are used, such as CuZn21Si3P (CW724R), which are slightly more difficult to machine.

💧
Dezincification. In certain types of water (hot, chloride-rich, or soft), brass alloys with a high zinc content can lose zinc from their surface: what remains is a reddish, porous, and brittle copper sponge, and the fillet may become loose or break. For plumbing applications, dezincification-resistant brass (containing a small amount of arsenic or specially treated) or bronze is used.
Example 21.7 · How much does a hexagonal brass bar weigh?

A 22-mm-sided (22-key) hexagonal bar made of CuZn39Pb3 is 3 m long. How much does it weigh?

Area of the hexagon with side length s: A = √32 · s² = 0.8660 · 22² = 0.8660 · 484 = 419.16 mm²
V = 419.16 × 3,000 = 1,257,469 mm³ ≈ 1.2575 dm³
m = 8.5 × 1.2575 = 10.69 kg
About 10.7 kg, or 3.56 kg per meter

Bronzes and Other Copper Alloys

I bronze sculptures Strictly speaking, these are copper alloys and stagnant (CuSn), containing 4% to 12% tin. They are more resistant to corrosion and wear than brass and have a low coefficient of friction compared to steel: it is the classic material used for bushings, bronze bearings, helical wheels for worm gears, and worm wheels for trapezoidal screws. It is called phosphor bronze A deoxidized bronze containing a small amount of phosphorus, which is more durable and elastic: CuSn8 (CW453K) for bushings and springs, CuSn12 (CC483K) for propeller wheel castings.

By extension, other copper alloys that do not contain zinc as their main component are also called "bronzes":

  • aluminum bronzes (CuAl10Fe5Ni5): very strong, almost as strong as quenched and tempered steel, excellent in seawater; marine propellers, pumps, and heavily loaded bushings;
  • cupronickel (CuNi10Fe1Mn, CuNi30Mn1Fe): copper and nickel, extremely resistant to seawater; used in the tubes of marine heat exchangers and desalination plants; coins are minted with 25% nickel;
  • nickel silver (copper, nickel, and zinc, CuNi18Zn20): silver-colored, used for keys, cutlery, and electrical contacts;
  • Beryllium copper (CuBe₂): After hardening, its tensile strength exceeds 1,200 N/mm²; used in springs, electrical contacts, and non-sparking tools for explosive environments (beryllium dust is toxic: do not dry-grind).
LeagueNumeric codeApproximate Rm (N/mm²)Typical Uses
Cu-ETP (semi-hard)CW004A250conductors, busbars, heat exchangers
CuZn37 (semi-hard)CW508L370sheet metal, tubes, deep-drawn workpieces
CuZn39Pb3CW614N430automatic turning, fillets, fasteners
CuZn21Si3PCW724R500lead-free plumbing
CuSn8 (phosphor bronze)CW453K450bushings, springs, shoulder washers
CuSn12 (cast)CC483K280helical gears, worm gears
CuAl10Fe5Ni5 (cast)CC333G650propellers, pumps, heavily loaded bushings
CuNi10Fe1MnCW352H300seawater pipes

Approximate, rounded values: These depend heavily on the condition (annealed, semi-hard, hard) and, for castings, on the type of casting.

Example 21.8 · Decoding Copper Abbreviations
CW614N: C for copper · W for plastic machining operations · 614 for the alloy number · N for the copper-zinc-lead group → it is CuZn39Pb3
CC483K: C for copper · C for cast · 483 · K for copper-tin alloy → this is CuSn12 for foundry use
CuAl10Fe5Ni5: copper (balance), approximately 10% aluminum, 5% iron, 5% nickel → aluminum bronze
The second letter indicates the product (W or C), and the last letter indicates the alloy family

21.6 Titanium and Its Alloys

Titanium is abundant in nature but difficult to extract: the ore is converted into titanium chloride, which is reduced with magnesium in a sealed furnace to produce a “sponge” that is then remelted under vacuum. The process is long and expensive, and titanium costs many times more than steel. It is chosen for three qualities combined:

  • Lightweight and strong: ρ ≈ 4.5 kg/dm³ (the Ti6Al4V alloy is around 4.4) and, in the Ti6Al4V alloy, Re ≈ 880 and Rm ≈ 950 N/mm²: it is as strong as a good quenched and tempered steel while weighing just over half as much;
  • exceptional corrosion resistance, even in seawater and many acids, thanks to an oxide layer similar to that of aluminum but much more stable;
  • Biocompatibility: The human body tolerates it, and bone grows by adhering to its surface.

The most commonly used types are commercially pure titanium (Grade 2), which is soft and highly corrosion-resistant, used in chemical plants and heat exchangers, and the Ti6Al4V alloy (Grade 5, containing approximately 6% aluminum and 4% vanadium), which is the most widely used: aeronautics (fasteners, carriages, compressor blades, fastening elements), biomedicine (hip and knee replacements, bone screws, dental implants; for these, the purest version, grade 23 or ELI, is used), motorsports, marine applications, and sporting goods. The elastic module is approximately 110,000 N/mm², half that of steel: a titanium workpiece bends more than an equivalent steel workpiece.

Because it's hard to work with

Titanium is classified in ISO Group S, along with superalloys (Chapter 24). There are three challenges:

  • It has low thermal conductivity (about one-seventh that of steel): the heat generated during cutting is transferred neither to the workpiece nor to the chips; instead, it remains concentrated at the tool tip and wears it down quickly;
  • It is chemically aggressive when hot: it reacts with the tool materials and tends to weld itself to the cutting edge;
  • Low elastic module: The workpiece gives way under the tool and then springs back, rubbing against the side of the tool and vibrating, especially if it is thin.

For this reason, machining is performed at low speeds (40 to 90 m/min for carbide turning, Table 26.12), with feeds that are not too small (to prevent scoring), sharp and rigid tools, abundant high-pressure coolant, and rigid machines and fixtures. Fine chips and titanium dust can catch fire: keep the work area clean and do not allow them to accumulate.

Example 21.9 · The Same Pass on Titanium and Aluminum

A Ø50 mm workpiece is turned for 100 mm at a feed rate of f = 0.2 mm/rev. For Ti6Al4V, the cutting speed is Vc = 60 m/min; for aluminum, it is 500 m/min. How long does the pass last in each case?

titanium: n = 1000 × 60 / (3.1416 × 50) = 381.97 rpm → t = Lf · n = 100 / (0.2 × 381.97) = 1.309 min = 78.5 s
aluminum: n = 1000 · 500 / (3.1416 · 50) = 3183.1 rpm → t = 100 / (0.2 · 3183.1) = 0.157 min = 9.4 s
ratio: 1.309 / 0.157 = 8.3 (the same ratio as the cutting speeds, 500 / 60)
With titanium, the machining process takes more than eight times as long; that's why titanium workpieces are so expensive to manufacture.

21.7 Magnesium, zinc, nickel, and other metals

Magnesium

Magnesium is the lightest of the structural metals: 1.74 kg/dm³, about two-thirds the density of aluminum. Its alloys with aluminum and zinc (such as AZ91 for die-casting and AZ31 for sheet metal and extrusions) are used for housings, frames of portable devices, steering wheels, and racing rims. It machines very well, but with one strict safety rule: fine chips and magnesium dust burn with a very white flame, and water on burning magnesium makes the fire worse. Work with coarse chips, sharp tools, no water-based emulsions (or use specific cutting fluids), closed containers for chips, and keep metal fire extinguishers (Class D) or dry sand near the machine.

Zinc and Zamak

Zinc (7.1 kg/dm³, melts at 420 °C) is used primarily to protect steel: galvanizing (hot-dip or electrolytic) coats bolts, sheet metal, and structures, and the zinc corrodes in place of the iron (Section 21.9). Zinc-aluminum alloys called zamak (ZP3, i.e., ZnAl₄, and ZP5, ZnAl₄Cu₁; approximately 6.7 kg/dm³) melt at around 385 °C and fill molds very well: through die-casting, they produce small, precise workpieces with thin walls and surfaces ready for chrome plating or painting, such as handles, locks, hinges, faucets, models, and small hardware. The molds last a very long time because they operate at low temperatures. However, zamak has low heat resistance and loses strength over time under load.

Nickel and Superalloys

Nickel (8.9 kg/dm³) is a key alloying element: it is found in austenitic stainless steels (Chapter 20), cupronickel alloys, and protective plating (nickel plating). Nickel superalloys, often known by trade names such as Inconel, maintain their strength up to 700 °C and beyond and resist hot oxidation: turbine blades, combustion chambers, and exhaust valves in racing engines. They are among the most difficult materials to machine (ISO Group S): extremely low cutting speeds and tools that wear out in just a few minutes.

White Metals for Bearings

White metals (or anti-friction metals) are soft alloys of tin or lead with antimony and copper, such as Sn89Sb8Cu3. They melt at low temperatures (around 240 °C) and are cast in a layer a few millimeters thick inside the steel shells of the plain bearings in large engines, turbines, and compressors. They are intentionally soft: small hard particles embedded in a soft mass that conforms to the shaft and “traps” dirt without scratching it. If the oil film is missing, the white metal melts before the shaft is damaged.

Cemented Carbide as a Material

Cemented carbide is not a cast alloy: it is a sintered material made of tungsten carbide (WC) grains held together by cobalt (Co), at a concentration of approximately 6% to 12%. It is extremely dense (about 14.5 kg/dm³, nearly twice that of steel), extremely hard, and has a module of elasticity of about 600,000 N/mm². In addition to inserts and milling cutters, which we will discuss in Chapter 25, it is used for anti-vibration bars, center drills, dies, stamping dies, and parts subject to heavy wear.

Materialρ (kg/dm³)Melting Point (°C)Main advantage
Magnesium and Alloys1,74-1,8650the lightest
Zama ZP36,7385Precision low-temperature die casting
Nickel8,91455corrosion and heat; the basis of superalloys
Inconel 718-type superalloy8,2around 1300temperature resistance above 650 °C
White metal Sn89Sb8Cu37,4about 240sliding, fits the shaft
WC-Co Cemented Carbide14-15It does not melt like a metal (it sintered)hardness and stiffness

Approximate and rounded values; for alloys, melting occurs over a range of temperatures.

Example 21.10 · A die-cast box made of three alloys

The body of a small box has a metal volume of 0.15 dm³. How much does it weigh when made of zamak, AlSi9Cu3 aluminum alloy, and AZ91 magnesium alloy?

zama: m = 6.7 × 0.15 = 1.005 kg
aluminum: m = 2.7 × 0.15 = 0.405 kg
magnesium: m = 1.8 × 0.15 = 0.270 kg
1.0 kg, 0.41 kg, and 0.27 kg: Zamak is chosen for its precision and finishing, certainly not for its weight

21.8 Specific Resistance: Which Metal Is Best?

Simply saying that titanium is “stronger” than aluminum isn’t enough: we need to ask how strong it is per unit of weight. The figure that tells us this is specific strength, the ratio of strength to density. It’s the criterion used to select materials for airplanes, race cars, bicycles, and robot arms—anything that moves and needs to be lightweight.

Specific resistance and specific stiffness
specific resistance = Rmρ specific stiffness = Eρ
Rm tensile strength in N/mm² (Re may also be used) · ρ in kg/dm³ · E elastic module in N/mm². With these units, the result is in kN·m/kg: (N/mm²) / (kg/dm³) = 106 N/m² / 103 kg/m³ = 103 N·m/kg.
Example 21.11 · Specific Resistance of Steel, Aluminum, and Titanium
quenched and tempered C45 steel: 700 / 7.85 = 89.2 kN·m/kg
quenched and tempered 42CrMo4 steel: 1000 / 7.85 = 127.4 kN·m/kg
6082-T6 aluminum: 310 / 2.7 = 114.8 kN·m/kg
7075-T6 aluminum (ρ = 2.8): 550 / 2.8 = 196.4 kN·m/kg
Titanium Ti6Al4V: 950 / 4.5 = 211.1 kN·m/kg
At the same weight, 6082 outperforms C45, while 7075 nearly matches titanium; titanium comes out on top, but only slightly over 7075
5010015020051S23551brass66PA689C45 (bon.)1156082-T612742CrMo4144AZ311967075-T6211Ti6Al4VRm / ρ (kN·m/kg)
Figure 21.5 · Specific resistance Rm/ρ. Steels are shown in gray, brass in yellow, polyamide in green, light aluminum and magnesium alloys in light blue, and titanium in red.

There is, however, a surprise. If you calculate the specific stiffness E/ρ, the three metals yield nearly the same value: steel 210,000 / 7.85 = 26,752, aluminum 70,000 / 2.7 = 25,926, titanium 110,000 / 4.5 = 24,444. This means that, for the same weight, none of the three is significantly stiffer than the others: anyone who wants a lightweight and stiff workpiece must focus on the shape (hollow sections, ribs, high beams; see Chapter 10) or switch to carbon-fiber composites.

Example 21.12 · A Light Tension Rod

A 1-meter-long tie rod must withstand a force of F = 30,000 N with a safety factor of 2 against yield. What is its weight in quenched and tempered C45, 6082-T6, 7075-T6, and Ti6Al4V?

C45: σam = 490 / 2 = 245 N/mm² → A = 30,000 / 245 = 122.45 mm² → V = 122.45 · 1000 = 0.1224 dm³ → m = 7.85 × 0.1224 = 0.961 kg
6082-T6: σam = 260 / 2 = 130 N/mm² → A = 230.77 mm² → m = 2.7 × 0.2308 = 0.623 kg
7075-T6: σam = 480 / 2 = 240 N/mm² → A = 125.00 mm² → m = 2.8 × 0.1250 = 0.350 kg
Ti6Al4V: σam = 880 / 2 = 440 N/mm² → A = 68.18 mm² → m = 4.5 × 0.0682 = 0.307 kg
0.96 kg, 0.62 kg, 0.35 kg, and 0.31 kg: Titanium weighs one-third as much as steel, but 7075 costs much less and weighs only 14% more

21.9 Galvanic Corrosion

When two different metals come into contact and are exposed to the same conductive liquid (saltwater, condensation, or rain mixed with dirt), they form a small battery. The less noble metal acts as the anode and corrodes more quickly than usual; the more noble metal acts as the cathode and remains protected. This is galvanic corrosion, and it ruins many fits made without a second thought: steel screws in copper sheets, aluminum rivets on stainless steel sheets, brass fillets on galvanized pipes.

To determine which metal is more noble, we use the galvanic series: metals arranged in order of their electrical potential, measured in a specific environment (usually seawater). The farther apart two metals are in the series, the stronger the battery.

+0.20.0−0.2−0.4−0.6−0.8−1.0−1.2−1.4−1.6voltgraphite+0.25titanium0.00passivated AISI 316 stainless steel−0.05nickel−0.1570/30 cupronickel−0.20bronzes−0.25copper−0.32brass−0.35unpassivated (active) stainless steel−0.50carbon steel and cast iron−0.65aluminum alloys−0.85zinc−1.03magnesium−1.60more noble(cathode)less noble(anode: corrodes)
Figure 21.6 · Simplified galvanic series in seawater, with indicative potentials in volts relative to a calomel reference electrode. The metals shown in red corrode when paired with those at the top.
Potential difference between two points
ΔU = Unoble − Uless noble
The potential of the two metals in the galvanic series, in volts. General rule of thumb: marine or aggressive outdoor environments up to 0.15 V; normal outdoor environments up to 0.25 V; dry, controlled indoor environments up to 0.50 V. Beyond these values, the pair should be isolated or avoided.

The ratio of the surface areas also matters. A small anode paired with a large cathode wears out quickly because all the current is concentrated on it: a steel screw in a large copper sheet will disappear in no time. The opposite case (small cathode, large anode) is much less problematic: a stainless steel screw in an aluminum sheet is acceptable, preferably if insulated. The golden rule: fasteners must be at least as corrosion-resistant as the workpieces they join.

Example 21.13 · Pairs to Avoid and Acceptable Pairs
aluminum and copper: ΔU = −0.32 − (−0.85) = 0.53 V → should be avoided; aluminum corrodes (bimetallic cable lugs are used)
aluminum and passivated stainless steel: ΔU = −0.05 − (−0.85) = 0.80 V → only with small stainless steel screws in large, isolated, and dry workpieces
steel and copper: ΔU = −0.32 − (−0.65) = 0.33 V → outdoors, steel rusts quickly when placed near copper
Brass and bronze: ΔU = −0.25 − (−0.35) = 0.10 V → acceptable almost everywhere
zinc and steel: ΔU = −0.65 − (−1.03) = 0.38 V → zinc acts as a sacrificial anode and protects the steel: this is the principle behind galvanizing and the use of sacrificial anodes on boats
Galvanic corrosion can also be put to good use: a less noble metal placed there on purpose protects the one that matters
🛡️
How to protect a fit. Choose metals that are close together in the series; insulate the two metals with plastic washers and bushings or with gaskets; paint both, or at least the cathode (painting only the anode is worse: every scratch becomes a tiny anode); keep water out using sealants and drainage holes.

21.10 Plastics and Engineering Polymers

Plastics (or polymers) are made up of very long molecules—called chains—formed by thousands of small, identical repeating units; almost all of them are derived from petroleum or natural gas. They are divided into three families based on how the chains are linked together.

thermoplasticfree-running chains: when heatedsoftens, remelts, and can be recycledthermosetDense network: rigid, does notremelts; burns when exposed to excessive heatelastomerfew cross-links between the chains:stretches and returns to its original shape
Figure 21.7 · The three families of polymers. The bonds between the chains (shown in red) determine how the material behaves when exposed to heat and under load.
  • Thermoplastics: The chains are separate and held together by weak forces. When heated, they soften and can be injection-molded, extruded, welded, and recycled. They include almost all plastics used in workshops. They can be amorphous (disordered chains, often transparent, such as PC and PMMA) or semicrystalline (partially ordered chains, opaque, more resistant to wear and solvents, such as POM, PA, PE, PTFE, and PEEK).
  • Thermosets: During production, the chains bond together to form a dense, permanent network (known as “cross-linking”). The workpiece is rigid, heat- and solvent-resistant, but cannot be remelted and is not easily recycled. Examples: phenolic resins (Bakelite, insulating laminates), epoxy resins (composite matrices, structural adhesives), unsaturated polyesters (fiberglass), and melamine resins.
  • Elastomers: tangled chains with few cross-links between them. They stretch significantly under load and return to their original shape: these are the rubbers used in gaskets, O-rings, belts, hoses, and vibration-damping mounts. The most commonly used in mechanical applications are NBR (nitrile rubber, resistant to mineral oils), FKM (fluoroelastomer, resistant up to about 200 °C and to aggressive oils), EPDM (water, steam, outdoor use; not resistant to oils), silicone (high and low temperatures), and polyurethane (extremely wear-resistant).

Engineering-Grade Technopolymers

Thermoplastics with mechanical properties good enough to replace metals in many workpieces—such as gears, bushings, slides, rollers, guides, and insulating workpieces—are called engineering plastics (or technical plastics). They come in the form of bars, sheets, and tubes to be machined on machine tools, or they are injection-molded in large production runs.

Materialρ (kg/dm³)Rm (N/mm²)E (N/mm²)Continuous Tmax (°C)α (10−6/°C)Water at 50% RH (%)Water at saturation (%)
POM-C (polyacetal)1,416528001001100,20,8
PA6 (polyamide, dry)1,1475300085902,89
PA66 (dry)1,1480320095852,58
PA6 + 30% glass fiber1,36160950011025 *2,06
PE-UHMW0,9320 (exasperating)70080200almost 0less than 0.1
PTFE (Teflon)2,225500260120almost 0almost 0
PEEK1,311003800250500,10,5
PC (polycarbonate)1,20652300115700,150,35
PMMA (Plexiglas)1,1970320080750,52

Approximate values at 23 °C, averaged and rounded, compiled by us; each manufacturer has its own. (*) Along the fibers; across the fibers, the expansion is much higher. For steel, as a comparison: ρ 7.85, E 210,000, α 11.5.

MaterialAdvantagesLimitationsTypical Uses
POM (polyacetal)rigid, dimensionally stable, smooth-running, excellent for use in machinesIt is sensitive to strong acids and burns easilygears, cams, bushings, precision workpieces, valves
PA6 and PA66 (polyamide, nylon)Tough, wear- and impact-resistant, and cost-effective; cast PA6 is produced in large workpiecesIt absorbs water and changes in size and stiffnesswheels, rollers, skids, large gears, pulleys
PE-UHMW (ultra-high-molecular-weight polyethylene)Exceptional resistance to wear and impact; non-slip; does not absorb watersoft, deforms under load, not very heat-resistantchain guides, hopper liners, conveyor belts
PTFE (polytetrafluoroethylene)Extremely low friction, resistant to almost all chemicals and temperatures ranging from −200 to +260 °C, insulatingsoft, “flows” under load (viscous flow), expensivegaskets, valve seats, insulation, nonstick coatings
PEEK (polyetheretherketone)Withstands temperatures up to 250 °C, steam, and chemicals; durable; biocompatibleextremely expensiveaeronautics, medical, workpieces for the chemical and food industries
PC (polycarbonate)transparent and nearly unbreakableIt scratches easily and is sensitive to solvents and certain lubricantsguards and windows for machine tools, covers
PMMA (polymethyl methacrylate)highly transparent, can be polished, weather-resistantprone to damage from impactsdisplay cases, signs, models, transparent lids
🪟
The machine’s guard is made of polycarbonate, not Plexiglas. If an insert breaks or a workpiece slips out of the vise, it strikes the glass plate with great force. Polycarbonate deforms but traps the fragment, while PMMA shatters. However, polycarbonate degrades when exposed to coolant; this is why the machine covers feature a polycarbonate sheet protected by a glass panel on the inside and must be replaced according to the manufacturer’s schedule.

Filled technopolymers

Fillers are often added to polymers. The most common are short glass fibers (15% to 50%): with 30% glass fiber, PA6 doubles its strength, triples its stiffness, expands much less, and withstands heat better; in exchange, it becomes less tough and is very abrasive to tools. The fibers align in the direction the plastic flows within the mold: the workpiece is stronger and expands less in that direction. Other fillers: carbon fiber (stiffness and conductivity), molybdenum disulfide and graphite (flowability), incorporated oil (self-lubricating bushings), and bronze in PTFE (reduced flow under load).

November 21: Thermal Expansion and Humidity

Plastics have two drawbacks that people coming from the metal industry tend to overlook: they expand significantly when heated, and some absorb moisture from the air and change size.

Thermal Expansion

The coefficient of thermal expansion for engineering polymers ranges from 50 to 200 × 10−6 /°C: 5 to 15 times that of steel. A plastic workpiece that heats up by a few degrees in a machine changes in size by tenths of a millimeter, and it fits with metal workpieces; it must take this into account, with larger clearances than those between metals.

Linear thermal expansion
ΔL = α · L · ΔT
ΔL change in length in mm · α coefficient of linear expansion in 1/°C · L initial length in mm · ΔT change in temperature in °C. This applies to all measurements of the workpieces: lengths, outside diameters, and hole diameters.
POM, length 150 mm, 20 to 60 °C+0.66 mmsteel, same length, same heating+0.069 mmend of the workpiece at 20 °CThe elongations (in red) are drawn magnified 75 times relative to the length of the workpieces.
Figure 21.8 · Two 150-mm-long workpieces heated from 20 to 60 °C: the POM stretches by 0.66 mm, while the steel stretches by less than 7 centimeters.
Example 21.14 · A workpiece of POM measured while hot

A workpiece of POM must be 80.00 mm long at 20 °C. It comes out of the machine at 35 °C, and the operator measures it immediately: the reading is exactly 80.00 mm. Is it acceptable?

ΔT = 35 − 20 = 15 °C
ΔL = 110 × 10−6 · 80 · 15 = 0.132 mm
At 20 °C, the workpiece will measure 80.00 − 0.132 = 79.868 mm
No: Once it cools down, it will be 0.13 mm shorter. Plastics are measured after they have returned to room temperature.

Moisture: Polyamide That Changes Size

Polyamides absorb water from the air until they reach equilibrium with the environment. Freshly produced PA6 is almost dry; in a warehouse with 50% relative humidity (RH), it eventually reaches about 2.8% water content, and when immersed in water, up to 9%. As it absorbs water, it swells and becomes more ductile but less rigid and less strong: the elastic module of conditioned PA6 drops to about 1200 N/mm², less than half that of dry PA6. For PA6, as a rough estimate, each percentage point of absorbed water causes the dimensions to increase by about 0.25%. POM absorbs very little water, while PE and PTFE absorb none at all; for this reason, when dimensions must remain stable in a humid environment, these materials are preferred over polyamide.

Growth due to water uptake (estimate)
ΔD = D · k · Δw100
ΔD change in dimension in mm · D initial dimension in mm · k increase in dimension, in %, for every 1% of water absorbed (for PA6, approximately 0.25; approximate value, depends on the type) · Δw increase in water content in percentage points
dry: Ø100.00wet (50% RH): Ø100.65Water absorption at 23 °C and 50% RH (%)PA62.8PA662.5PA6 + 30% glass2.0POM0.20PC0.15PEEK0.10PE-UHMWnearly 0
Figure 21.9 · On the left, a dry-machined PA6 ring with a diameter of 100: the hatched area shows its dimensions after absorbing moisture from the environment (enlarged illustration of the expansion). On the right, the water absorbed by certain engineering polymers at 23 °C and 50% RH; values are approximate.
Example 21.15 · How much does a PA6 ring expand?

A PA6 ring is turned to a diameter of 100.00 mm from a nearly dry bar (0.2% water). Over time, in the workshop at 50% relative humidity, its water content reaches 2.8%. What will its diameter be? And what if it were machined while submerged in water (9%)?

In the workshop: Δw = 2.8 − 0.2 = 2.6 points → ΔD = 100 · 0.25 · 2.6 / 100 = 0.65 mm → Ø100.65
in water: Δw = 9 − 0.2 = 8.8 points → ΔD = 100 · 0.25 · 8.8 / 100 = 2.2 mm → Ø102.2
More than half a millimeter just from atmospheric humidity: a tolerance of one hundredth on a polyamide makes no sense
💡
How to address this issue. For precision workpieces in humid environments, choose POM, PE-UHMW, or PEEK instead of polyamide. If polyamide is required, allow for generous clearances (PA bushings are installed with much more clearance than a bronze bushing) or machine the workpieces after they have been conditioned—that is, after allowing them to stabilize in the environment where they will be used.

21.12 Plastics in Machine Tools

Plastics can be cut with little force, but they have their own characteristics because they are soft, elastic, insulating, and melt at low temperatures.

  • Extremely sharp, positive cutting edges with large rake angles: tools made of high-speed steel or polished carbide are used—the same as for aluminum. A dull cutting edge does not cut; it crushes, heats, and tears.
  • Heat is the enemy: plastic is a poor conductor, so heat remains in the cutting zone and the material softens, sticks to the tool, or melts. Use generous feeds (it’s better to have a thick chip than a thin one that causes friction) and cool with compressed air, water, or a clean emulsion.
  • Light, evenly distributed clamping: the workpiece deforms in the vise or spindle and, when released, returns to its original shape, eliminating the tolerance. Wide or soft jaws, sector jaws, and open-face clamps are used for slabs.
  • Internal stresses: Extruded bars and plates have stresses that are released when a significant amount of material is removed. For precision workpieces, rough-machine the workpiece, let it rest (or anneal it, if recommended by the supplier), and then finish it.
  • Be careful with lubricants: PC and PMMA can crack when they come into contact with certain oils and solvents (stress cracks); if in doubt, use air or water.
  • Safety: PTFE heated above 400 °C releases harmful fumes; dust from materials filled with glass or carbon must be vacuumed up.
MaterialTurning speed (m/min)f (mm/revolution)Notes
POM200-5000,1-0,4The easiest: continuous chips, consistent dimensions
PA6 and PA66200-5000,1-0,4Long, tough chips—you'll need a chip breaker
PE-UHMW150-4000,1-0,5very soft and elastic, with an extremely cutting edge blade
PTFE100-3000,05-0,25slips under the clamp; difficult measurements
PEEK150-3000,05-0,25hard metal, cool; very expensive material
PC and PMMA150-3000,05-0,2Fragile: minimal feed at the exit; final polishing
Filled with glass100-2500,1-0,3abrasives: carbide or PCD

Approximate starting values, rounded, compiled by us. In milling, single- or double-edged cutters with highly polished grooves are used.

Example 21.16 · Turning a POM Bushing

A POM bushing with a diameter of 50 mm is turned at Vc = 300 m/min with a feed rate of f = 0.2 mm/rev. How many revolutions are required, and what should be entered in the program?

n = 1000 · 3003,1416 · 50 = 1909.9 rpm ≈ 1910 rpm
with constant cutting speed: G96 S300 with limit G50 S3000 (Siemens: LIMS=3000), feed rate G95 F0.2
Compressed-air cooling; final measurement after the workpiece has returned to room temperature
Approximately 1910 rpm at Ø50

21.13 Composite Materials and 3D Printing

Composites

A composite material combines two different materials to achieve something that neither of them can achieve on its own. In mechanical engineering, composites include:

  • the load-bearing fibers: carbon fiber (extremely stiff and strong, lightweight, expensive), fiberglass (inexpensive, less stiff, insulating), aramid fiber (extremely tough, used for ballistic protection);
  • the matrix, which is almost always a thermosetting epoxy or polyester resin, holds the fibers in place, protects them, and transfers the load from one fiber to another.

The most important characteristic of long-fiber composites is anisotropy: their properties are not the same in all directions. Along the fibers, the material is extremely strong; across the fibers, it is almost entirely the resin that matters. For this reason, workpieces are made by layering many thin sheets with the fibers oriented in different directions (0°, 90°, ±45°), chosen according to the loads.

cross-section of a layercircles = cut fibers, background = matrixlayer at 0°90° layerlayer at +45°layer at −45°cross-ply laminateEach layer is strong only along its grain
Figure 21.10 · On the left is a cross-section of a layer: the fibers (about 60% of the volume) are embedded in the resin. On the right are four layers with fibers oriented in different directions, stacked one on top of the other.
Rule of Mixtures
ρc = Vf · ρf + (1 − Vf) · ρm E∥ = Vf · Ef + (1 − Vf) · Em
1E⊥ = VfEf + 1 − VfEm
Vf: fiber volume fraction (0 to 1) · ρf, ρm, ρc: densities of the fibers, matrix, and composite in kg/dm³ · Ef, Em: elastic modules of the fibers and matrix in N/mm² · E∥: module along the fibers · E⊥: transverse module (simple estimate)
Example 21.17 · How stiff is a carbon-fiber composite?

A unidirectional layer consists of 60% carbon fiber (ρ = 1.8 kg/dm³, E = 230,000 N/mm²) embedded in epoxy resin (ρ = 1.2 kg/dm³, E = 3,000 N/mm²).

ρc = 0.6 × 1.8 + 0.4 × 1.2 = 1.08 + 0.48 = 1.56 kg/dm³
along the fibers: E = 0.6 × 230,000 + 0.4 × 3,000 = 138,000 + 1,200 = 139,200 N/mm²
Shear: 1/E = 0.6 / 230,000 + 0.4 / 3,000 = 0.0000026 + 0.0001333 → E = 7,356 N/mm²
specific stiffness along the fibers: 139,200 / 1.56 = 89,231, compared to about 26,000 for metals
Along the fibers, it is 19 times stiffer than across them, and for the same weight, it is more than three times stiffer than steel

Composites are challenging to machine: carbon and glass fibers wear down tools like a grinding wheel, and the layers tend to delaminate (split open) and fray at the entry and exit points of the holes. Diamond-coated carbide or PCD tools are used, along with specialized geometries, supports beneath the holes, and effective dust extraction, as the dust is irritating and, in the case of carbon dust, conductive (which can damage the machine’s electronics).

3D Printing of Polymers

3D printing (additive manufacturing) builds the workpiece layer by layer instead of removing material. For polymers, the most common techniques are: fused deposition modeling (FDM), using materials such as PLA, PETG, ABS, and carbon-fiber-reinforced polyamides; stereolithography (SLA) using liquid resins, for highly detailed workpieces; and laser sintering (SLS) of PA12 polyamide powders, for functional workpieces without support structures. Printed workpieces are also anisotropic: adhesion is weaker between layers, so a workpiece is less resistant when pulled in the direction of construction. The techniques, limitations, and metal printing are discussed in Chapter 23.

21.14 Choosing the Material

Choosing the material for a workpiece means balancing requirements that are often at odds with one another. It’s best to ask the right questions in the right order and gradually rule out the materials that aren’t suitable.

CriterionA question to ask yourselfFavorite Materials
ResistanceWhat kind of loads does it carry? Do you need an R?e High strength or fatigue resistance?quenched and tempered steels, titanium, 7075
StiffnessHow much can it bend?steel and cast iron (high E); carbon composites
WeightDoes the workpiece move, accelerate, or can it be moved by hand?aluminum, magnesium, titanium, plastics, composites
EnvironmentHumidity, seawater, chemicals, temperature?stainless steel, bronze, cupronickel, titanium, 5083, PTFE, PEEK
Friction and WearDoes it rub against other workpieces? Without lubricant?bronze, non-ferrous metals, POM, PA, PE-UHMW, PTFE
ConductivityIs it meant to conduct electricity or heat, or to insulate?copper, aluminum; for insulating plastics and anodizing
WorkabilityHow many workpieces? What machines? What is the cycle time?CuZn39Pb3 brass, 2011, free-cutting steels, POM
CostHow much do the materials and machining operations cost?unalloyed steels, 6082, PA6

The cost of materials is calculated per workpiece, not per kilogram: a lightweight metal that is expensive per kilogram may cost little per workpiece, because you buy less of it for the same volume. And the cost of materials is added to the cost of machining operations, which are often the largest expense for a turned workpiece (Chapter 30).

Example 21.18 · Selecting the Alloy for a Turned Workpiece

A compressed air fitting is mass-produced on an automatic sliding-head lathe. Each workpiece has 12 cm³ of gross material (0.012 dm³). It must withstand the moisture in the line, have a precise thread, and the purchasing department is requesting the cost of the material. Sample prices, for calculation purposes only: brass 7 €/kg, alloy 2011 5 €/kg, free-cutting steel 11SMnPb30 1.5 €/kg.

CuZn39Pb3 brass: m = 8.5 × 0.012 = 0.1020 kg → 0.1020 × 7 = 0.714 € per workpiece
2011-T3 aluminum: m = 2.7 × 0.012 = 0.0324 kg → 0.0324 × 5 = 0.162 € per workpiece
11SMnPb30 steel: m = 7.85 × 0.012 = 0.0942 kg → 0.0942 × 1.5 = 0.141 € per workpiece
Steel: the least expensive option, but it rusts; it requires zinc or nickel plating, which is costly and adds to the production time
2011: Inexpensive and very lightweight, with short chips, but it has low corrosion resistance: it must be anodized, and the threads are more delicate
Brass: the most expensive material, but it’s the fastest to machine, requires no additional treatment, and the chips sell well
For a pneumatic fillet, the standard choice is CuZn39Pb3 brass (which may be nickel-plated for aesthetic reasons); anodized 2011 aluminum is chosen when weight is a factor
🖥️
Try it out in the simulator. In the CNC Code’s lathe and milling machine, you can write the same programs using the spindle speeds for aluminum, brass, or titanium and compare cycle times: it’s the fastest way to understand how much the material affects the cost of a workpiece.

9:15 p.m. The formulas in this chapter

WhatFormula
Mass of a workpiecem = ρ · V (kg, kg/dm³, dm³)
Same workpiece, different materialsm2 / m1 = ρ2 / ρ1
Anodizing: Increase in DiameterΔD = 2 · (outward fraction) · thickness
Resistance of a ConductorR = L / (σ · A) (Ω, m, MS/m, mm²)
Strength and Specific StiffnessRm / ρ · E / ρ (kN·m/kg, where N/mm² and kg/dm³)
Galvanic coupleΔU = Noble − Less Noble
Thermal ExpansionΔL = α · L · ΔT
Moisture-induced expansion (PA6, estimate)ΔD = D · k · Δw / 100, where k ≈ 0.25
Rule of Mixturesρc = Vf · ρf + (1 − Vf) · ρm · E∥ = Vf · Ef + (1 − Vf) · Em
Spindle speedn = 1000 · Vc / (π · D)

21.16 Exercises

Use the densities shown in Figure 21.1 and the data from the tables in this chapter. Try it on your own before looking at the solution.

Exercise 1. A round bar with a diameter of 30 mm and a length of 2 m: How much does it weigh when made of 6082 aluminum alloy, and how much when made of brass?
Solution

V = π/4 · 30² · 2000 = 1,413,717 mm³ = 1.4137 dm³. Aluminum: 2.7 × 1.4137 = 3.82 kg. Brass: 8.5 × 1.4137 = 12.02 kg.

Exercise 2. What do EN AW-5754-H22 and EN AW-6061-T651 mean?
Solution

5754-H22: 5000 series (magnesium) alloy for machining operations, not heat-treatable, work-hardened, and then partially annealed to one-quarter hardness; suitable for sheet metal bending and humid environments. 6061-T651: 6000 series (magnesium and silicon), solution-treated, quenched, artificially aged, and stretch-relaxed; suitable for milling plates.

Exercise 3. Calculate the specific strength of 2011-T3 aluminum (Rm = 330 N/mm²) and S355 steel (Rm = 510 N/mm²). Which is more suitable for the same weight?
Solution

2011: 330 / 2.7 = 122.2 kN·m/kg. S355: 510 / 7.85 = 65.0 kN·m/kg. For the same weight, the 2011 has nearly twice the strength.

Exercise 4. A PA6 bushing is turned to a dry fit with an outside diameter of 60.00 mm (0.2% water content) and swells to 2.8% during service. By how much does the diameter increase (k = 0.25)?
Solution

Δw = 2.6 points; ΔD = 60 × 0.25 × 2.6 / 100 = 0.39 mm: the diameter becomes approximately 60.39 mm.

Exercise 5. A 250-mm-long POM guide rod is heated from 20 to 50 °C. How much does it expand? What about an identical steel guide rod?
Solution

POM: 110 · 10−6 · 250 · 30 = 0.825 mm. Steel: 11.5 · 10−6 · 250 · 30 = 0.086 mm. POM stretches nearly ten times as much.

Exercise 6. Using the series shown in Figure 21.6, calculate the potential difference for the steel-copper and magnesium-steel pairs. Which one corrodes?
Solution

Steel and copper: −0.32 − (−0.65) = 0.33 V; the steel corrodes. Magnesium and steel: −0.65 − (−1.60) = 0.95 V; the magnesium corrodes (it is used as a sacrificial anode in water heaters).

Exercise 7. A Ti6Al4V pin with a diameter of 25 mm is turned at a cutting speed (Vc) of 50 m/min. How many revolutions?
Solution

n = 1000 · 50 / (3.1416 · 25) = 636.6 rpm, approximately 637 rpm.

Exercise 8. A layer of fiberglass-reinforced plastic consists of 50% glass fiber (ρ = 2.55 kg/dm³, E = 72,000 N/mm²) embedded in resin (ρ = 1.2 kg/dm³, E = 3,000 N/mm²). Calculate ρ and the module of elasticity in the fiber direction.
Solution

ρ = 0.5 · 2.55 + 0.5 · 1.2 = 1.875 kg/dm³. E = 0.5 × 72,000 + 0.5 × 3,000 = 37,500 N/mm², about half that of aluminum.

Exercise 9. A Ø20.000 mm hole in a workpiece of aluminum is given a standard anodization coating of 25 μm, one-third of which grows outward. What will be the diameter of the hole after the treatment?
Solution

Increase in radius = 25 / 3 = 8.33 μm; increase in diameter = 16.7 μm, toward the center of the hole. The hole becomes Ø20.000 − 0.017 = 19.983 mm.

Exercise 10. A copper conductor has a cross-sectional area of 16 mm². What cross-sectional area must an aluminum conductor have to have the same resistance (σCu = 58, σAl = 35 MS/m)?
Solution

AAl = 16 × 58 / 35 = 26.51 mm²; in practice, the next larger commercially available cross-sectional area is chosen.

Exercise 11. A plate must support the same load in 6082-T6 (Re = 260 N/mm², ρ = 2.7) or in 7075-T6 (Re = 480 N/mm², ρ = 2.8). How much larger a cross-sectional area is required for 6082, and how much more does it weigh?
Solution

The cross-sectional areas are inversely proportional to the yield strengths: 480 / 260 = 1.846, which is 85% more cross-sectional area. The masses: (2.7 / 260) / (2.8 / 480) = 1.78, meaning the 6082 weighs 78% more.

Exercise 12. A workpiece of aluminum measures 150.040 mm at 28 °C. How long will it be at 20 °C (α = 23 × 10−6 /°C)? If the dimension specified in the drawing is 150,000 ± 0.02, is the workpiece acceptable?
Solution

ΔL = 23 × 10−6 · 150 · 8 = 0.0276 mm; at 20 °C, it measures 150.040 − 0.028 = 150.012 mm. Yes, it’s within tolerance (when measured while hot, it seemed to be outside).