Chapter 22

Heat Treatments and Surface Treatments

The same steel can be as soft as mild iron or as hard as a file: it depends on how it is heated and how it is cooled. Heat treatments change the internal structure of the metal without altering its composition; surface treatments affect only the outer layer of the workpiece. In this chapter, we’ll explore what happens inside steel, how to select a treatment, how to specify it on a drawing, and how to organize the processing cycle for a workpiece to be treated.

22.1 Why Are Steels Treated?

A gear shaft must be hard on the surface—where the gears and bearings engage—but tough on the inside, so it doesn’t break under impact. A high-torque fastener must be strong but not brittle. A die must withstand wear and tear over hundreds of thousands of workpieces. No steel, as it comes straight from the steel mill, possesses all these qualities at once: heat treatment is what gives them these properties.

A heat treatment is a cycle consisting of heating, holding at a specific temperature, and cooling at a selected rate. No material is added or removed (except in thermochemical treatments, which introduce carbon or nitrogen into the surface); only the arrangement of the iron and carbon atoms—that is, the structure—changes. With this treatment, it is possible to:

  • to harden the workpiece so that it can withstand wear and loads (hardening);
  • make him tenacious and strong at the same time, eliminating the brittleness caused by heat treatment (tempering, quenching and tempering);
  • to soften it so it can be machined more easily with tools (annealing);
  • to relieve stresses caused by welding, cold deformation, or heavy roughing (stress relief);
  • to make the grain uniform after forging or rolling (normalization);
  • to harden only the surface, leaving the core soft (surface hardening, case hardening, nitriding).
85060020 heating holding hardening tempering coolingin air heat treatment = hardening + high-temperature tempering temperature (°C)time
Figure 22.1 · A heat treatment cycle for structural steel: heating, holding at 850 °C, quenching, followed by tempering at 600 °C. Times and temperatures are approximate.

To understand which test cycle to use, you need to know what happens inside the steel when it is heated. That is the focus of the next two paragraphs. The tests used to measure the results—particularly the Rockwell (HRC), Vickers (HV), and Brinell (HB) hardness tests—are explained in Chapter 19; the steel grades and their designations are covered in Chapter 20.

22.2 Steel Structures

Steel is iron with a small amount of carbon—usually between 0.1 and 1 percent—plus other alloying elements. The iron atoms are arranged in an orderly lattice, like oranges in a crate, and the shape of this lattice changes with temperature. Carbon, which is a much smaller atom, slips into the spaces between the iron atoms. Depending on how it is arranged, this gives rise to the five structures you need to know:

  • ferrite (α-iron): This is the form of iron at room temperature. It dissolves very little carbon (at most 0.02%), and is soft, ductile, and magnetic. Its hardness is approximately 80–90 HB.
  • cementite (Fe₃C): a compound of iron and carbon containing 6.67% C. It is extremely hard and brittle, with a hardness of approximately 800 HV. It is not used on its own, but it is what gives steel its hardness.
  • Perlite: It is not a phase but a mixture of extremely thin lamellae of ferrite and cementite, alternating like the pages of a book. It forms when austenite containing 0.77% carbon cools slowly. Under a microscope, after acid etching, it exhibits a mother-of-pearl luster, hence its name. It is harder and more durable than ferrite (approximately 200–250 HB when finely lamellar).
  • Austenite (γ-iron): It exists in common steels only at high temperatures, above 727 °C. Its crystal lattice has more space between the atoms and can dissolve a large amount of carbon, up to 2.11%. It is not magnetic. It is the starting point for all heat treatment: first, the entire material is transformed into austenite, and then the cooling method is determined.
  • martensite: It forms when austenite is cooled so quickly that the carbon does not have time to precipitate out to form cementite. It remains trapped in the iron lattice and distorts it, resulting in a needle-like structure that is extremely hard and brittle. This is the structure of hardened steel.
ferritesoft and ductileperliteferrite lamellae and Fe₃Cferrite + perliteannealed C45austeniteonly at high temperaturesmartensiteneedles, very hard
Figure 22.2 · Schematic representation of how the following appear under a microscope: ferrite grains, pearlite lamellae, the ferrite-pearlite mixture in annealed C45 steel, austenite grains (only when hot), and martensite needles.

Between pearlite and martensite lies an intermediate structure called bainite: it forms when the workpiece cools quickly enough to prevent the formation of pearlite, but is kept at a temperature (between about 250 and 550 °C) at which martensite has not yet formed. It is less hard than martensite but very tough.

The hardness of martensite depends almost entirely on carbon: the more carbon there is, the more the crystal lattice is distorted, and the harder the martensite is. Alloying elements serve primarily another purpose, namely to induce the formation of martensite even with less rapid cooling (Section 22.6). An empirical formula, valid up to about 0.5% carbon, gives the hardness of fully developed martensite:

Maximum martensite hardness (approximate)
HRCmax ≈ 20 + 60 · √C
HRCmax Rockwell C hardness of fully martensitic steel immediately after quenching · Carbon content (C) in mass percent (0.45 for C45). Above 0.6% carbon, the hardness no longer increases and stabilizes at around 64–66 HRC.
Example 22.1 · How hard does it become after quenching?

What is the maximum hardness that martensite in C45 steel (0.45% C) can reach? And what about that of a case-hardened steel (0.2% C)? And that of C10 steel?

C45: HRC ≈ 20 + 60 · √0.45 = 20 + 60 · 0.6708 = 20 + 40.2 = 60.2 HRC
0.2% C: HRC ≈ 20 + 60 · √0.2 = 20 + 60 · 0.4472 = 46.8 HRC
C10: HRC ≈ 20 + 60 · √0.1 = 20 + 60 · 0.3162 = 39.0 HRC
C45 approx. 60 HRC · 0.2% C approx. 47 HRC · C10 approx. 39 HRC

In practice, a workpiece of water-hardened C45 steel reaches 55–58 HRC, because martensite formation is never 100 percent complete. C10 steel is almost never water-hardened: the martensite would be too soft, and, more importantly, it would require such rapid cooling that no actual workpiece of steel can achieve it. To harden low-carbon steels, carbon is added to the surface through case hardening (section 22.10).

22.3 The iron-carbon diagram

The iron-carbon phase diagram shows the structure of steel at equilibrium for each carbon content and temperature. “At equilibrium” means under conditions of very slow heating and cooling: this is the starting point, which is then deliberately “deviated from” by the rapid cooling of the quenching process. The complete drawing extends up to 6.67% carbon and also includes cast irons; here we are showing only the portion for steels, up to about 2%.

6007008009001,0001,1005000.51.01.52.000.77S (0.77% C; 727 °C)A1 · 727 °CA3Acm912austenite (γ)ferrite +austeniteaustenite +cementiteferrite + perliteperliteperlite + cementiteC45C60C100temperature (°C)carbon (% by mass)
Figure 22.3 · Simplified iron-carbon diagram (rounded values: A1 at 727 °C, A3 from 912 to 727 °C, Acm from 727 °C to 1148 °C at 2.11% C, drawn as a straight line). The quenching temperatures for C45, C60, and C100 are shown in red.

The three key points are as follows:

  • A1, the horizontal line at 727 °C: there is no austenite below this temperature. When steel is heated beyond A1, pearlite transforms into austenite.
  • A3, the line that runs from 912 °C (pure iron) to 727 °C: above A3, steels with less than 0.77% carbon are all austenitic. Between A1 and A3, there is a mixture of ferrite and austenite.
  • ACM, the line rising to the right: above the ACM, steels with more than 0.77% carbon are all austenite; below it, there is austenite plus cementite.

The three lines intersect at the eutectoid point S, at 0.77% carbon and 727 °C. A steel with exactly 0.77% carbon is called eutectoid, and when cooled slowly, it transforms entirely into pearlite. Those with less carbon (almost all structural steels: C40, C45, 42CrMo4, 39NiCrMo3) are hypoeutectoid and, when cold, consist of ferrite and perlite; those with more carbon (tool and bearing steels, such as C100 or 100Cr6) are hypereutectoid and, when cold, consist of perlite and cementite.

The Rule for Quenching Temperature

To harden steel, you must first transform it into austenite: this is called austenitization. The rule of thumb is:

  • hypoeutectoid steels: A3 + 30–50 °C. Below A3, some ferrite would remain, which does not harden and leaves soft spots; if the temperature is too high, the grain size increases and the workpiece becomes brittle;
  • Hyper-eutectoid steels: A1 + 30–50 °C, not above Acm. A small amount of undissolved carbides is intentionally left behind; these are extremely hard and help resist wear. Heating above Acm would cause the grain size to increase and leave too much untransformed austenite after quenching.

To read A3 without a ruler or set square, you can use a formula that approximates the curve in our diagram (this is an approximation designed to pass through 912 °C and 727 °C; it is not a physical law):

Line A3 and hardening temperature (simplified diagram)
A3 ≈ 912 − 211 · √C
Ttempering = A3 + (30 ÷ 50) °C or, if C > 0.77%, Ttempering = 727 + (30 ÷ 50) °C
A3: temperature of line A3 in °C · C: carbon content in mass %, from 0 to 0.77 · Ttempra: austenitizing temperature in °C. The symbol ÷ indicates a range: add 30 to 50 °C.
Example 22.2 · Hardening Temperature of C45

A C45 pin (0.45% C) needs to be hardened. What temperature should the furnace be set to?

A3 ≈ 912 − 211 · √0,45 = 912 − 211 · 0,6708 = 912 − 141,5 = 770,5 °C
Ttempering = 770.5 + 30 = 800.5 °C up to 770.5 + 50 = 820.5 °C
From the diagram: approximately 800–820 °C

The manufacturers' data sheets for water-hardened C45 indicate slightly higher values, around 820–860 °C. The reason is that the diagram applies to iron containing only carbon: the silicon and manganese in actual steel shift the lines slightly, and with real workpieces, you want to be sure that all the ferrite has disappeared. The rule is meant to help you understand and verify; when a manufacturer’s specification is available, follow it.

Example 22.3 · C60 and C100

What are the quenching temperatures indicated by the phase diagram and the rule of thumb for a C60 (0.60% C) and a C100 (1.0% C)?

C60: A3 ≈ 912 − 211 · √0,6 = 912 − 211 · 0,7746 = 912 − 163,4 = 748,6 °C
C60: Ttempering = 748.6 + 30 ÷ 50 = 778.6 to 798.6 °C, approximately 780–800 °C
C100 is hypereutectoid: Ttempering = 727 + 30 ÷ 50 = 757 to 777 °C
Verification: For C = 1.0, the Acm value in the diagram is 727 + 314 · (1.0 − 0.77) = 727 + 72.2 = 799 °C, and 777 °C is below it ✓
C60: approximately 780–800 °C · C100: approximately 760–780 °C

The more carbon there is, the lower the quenching temperature—up to 0.77%; beyond that, the temperature remains fixed at A1. Here, too, the actual data sheets show slightly higher values (for C60, approximately 800–840 °C).

22.4 Heating and Holding in the Oven

The workpiece does not become austenite the moment the furnace reaches the correct temperature. First, it must heat through to the core; then it must remain at that temperature long enough for the transformation to complete and for the carbon to distribute evenly. The total time is called the holding time and depends on the thickness of the workpiece, the furnace, the load, and the steel: alloy steels contain carbides that dissolve more slowly and require more time.

For an initial estimate, a rule of thumb is used, which should be considered only as a guideline:

Baking time (as a general guideline)
t ≈ k · s
t: time in minutes, counted from the moment the furnace returns to temperature after the batch has been loaded · s: thickness of the thickest part in mm (for a round bar, the diameter) · k approximately 1 min/mm for unalloyed steels, approximately 1.5 min/mm for alloyed steels, with a minimum of approximately 20 minutes. For very large workpieces or fully loaded furnaces, this time is extended; the correct values are provided in the furnace and steel data sheets.
Example 22.4 · How long should it stay in the oven?

I am heat-treating two Ø60 shafts: one made of C45 and one made of 42CrMo4. How long should they remain at that temperature?

C45: t ≈ 1 × 60 = 60 min
42CrMo4: t ≈ 1.5 × 60 = 90 min
About 1 hour for C45 and 1½ hours for 42CrMo4, starting from the moment the furnace reached the desired temperature

During the holding period, if air is present in the furnace, the carbon on the surface reacts with oxygen and is removed: this is decarburization. The decarburized layer, which is a few hundredths to a few tenths of a millimeter deep, remains soft after quenching, and a layer of oxide scale (calamine) also forms beneath it. To prevent this, controlled-atmosphere furnaces (protective gases), vacuum furnaces, or molten salt baths are used; otherwise, an allowance of metal is left, which is removed during grinding (section 22.14).

How much does an oven cycle cost?

The heat required to warm the load is calculated using the calorimetry formula. The amount of electricity consumed is higher because some of the heat is lost through the walls and doors; this is reflected in the heating efficiency. Furthermore, while the workpiece remains at temperature, the furnace continues to consume energy to compensate for these losses.

Energy Consumed During a Furnace Cycle
Q = m · c · ΔT3600 E = Qη + Pd · tp
Q heat entering the load, in kWh · m mass of the load (workpieces and baskets) in kg · c average specific heat of steel between 20 and 850 °C, approximately 0.6 kJ/(kg·K) (approximate value) · ΔT temperature difference in K (equal in °C) · 3600 kJ = 1 kWh · η heating efficiency; for an electric furnace, approximately 0.5 · Pd power lost through the walls during the holding period, in kW · tp holding time in hours · E electrical energy in kWh
Example 22.5 · Energy and Cost of a Heat Treatment

An electric furnace heats 200 kg of workpieces (40 workpieces weighing 5 kg each) from 20 to 850 °C. Heating efficiency: 0.5; heat loss during holding: 8 kW per hour; energy cost: 0.25 €/kWh.

ΔT = 850 − 20 = 830 K
Q = 200 × 0.6 × 830 / 3,600 = 99,600 / 3,600 = 27.7 kWh
E = 27.7 / 0.5 + 8 × 1 = 55.3 + 8 = 63.3 kWh
cost = 63.3 × 0.25 = 15.83 € · per workpiece 15.83 / 40 = 0.40 €
About 63 kWh and €16 in energy costs per charge, 40 cents per workpiece

Added to this are the cost of the discovery (a second, lower furnace cycle), the protective gas, the quenching medium, labor, and furnace depreciation. That is why heat treatment providers charge by the kilogram and on a full-load basis: a half-empty furnace costs almost as much as a full one.

22.5 Cooling: TTT and CCT Curves

Once the workpiece is entirely austenite, the cooling process determines the final microstructure. If it cools slowly, the carbon has time to redistribute, and pearlite forms (along with ferrite or cementite, depending on the carbon content); if it cools quickly, the pearlite becomes increasingly fine, and then bainite appears; if it cools quickly enough, martensite forms.

These transformations can be seen in two types of diagrams, which every steel manufacturer publishes for its materials:

  • The TTT curve (time, temperature, transformation), also known as the isothermal transformation curve: the sample is rapidly heated to a certain temperature, held there, and the time it takes for the austenite to begin and complete its transformation is observed. It is shaped like a “C” (or a nose), with the tip pointing to the left;
  • the CCT curve (continuous cooling transformation): The sample cools continuously, just as it does during actual quenching. It has a similar shape, shifted slightly to the right and downward. This is the most useful one in the workshop.
1002003004005006007008009000.111010010³10⁴10⁵A1 727 °CMsMfmartensiteaustenitepearlitebainitewateroilairoventemperature (°C)time (s, logarithmic scale)
Figure 22.4 · Schematic C-curve for a steel such as C45 (solid line: start of transformation; dashed line: end). The colored curves represent cooling rates from 850 °C: water, critical rate (red dashed), oil, air, and furnace. Time is on a logarithmic scale; the values are only qualitative.

The cooling curves for the workpieces are plotted on top of each other in the diagram. Here's how to read it:

  • Water cooling passes to the left of the tip of the C curve without touching it: the austenite reaches the Ms line (the start of martensite) intact and transforms into martensite, completing the transformation below the Mf line. This is hardening;
  • In oil quenching, for a low-alloy steel such as C45, the temperature approaches the critical point and passes through it: part of the austenite transforms into fine pearlite or bainite, and the workpiece remains less hard;
  • Cooling in still air passes through the C phase at the top: fine perlite and ferrite. This is normalization;
  • Cooling in the turned-off furnace causes the temperature to rise even higher: coarse perlite, the softest structure. This is annealing.

The Critical Quenching Speed

The cooling curve that just grazes the tip of the C, without crossing it, is called the critical hardening rate: it is the minimum rate required to obtain all martensite. Every steel has its own. In unalloyed steels, the tip of the C is far to the left (less than one second) and the critical speed is extremely high: only water can achieve it, and only on thin sections. Alloying elements (chromium, molybdenum, nickel, manganese) shift the C curve to the right: the critical speed decreases, and oil, compressed air, or even still air are sufficient.

Average cooling rate
v = T1 − T2Δt
v: average cooling rate in °C/s · T1: initial temperature in °C · T2: final temperature in °C · Δt: time elapsed in s
Example 22.6 · Why C45 steel in oil does not harden through

In general terms, the tip of the “C” in C45 reaches approximately 550 °C after about 1 s; that of 42CrMo4 reaches about 500 °C after about 10 seconds. The core of a medium-diameter bar quenched in oil cools from 850 to 500 °C in about 12 seconds. What happens to the two steels? (These are rough estimates, just to get the idea.)

C45, starting at 830 °C: vcrit ≈ (830 − 550) / 1 = 280 °C/s
42CrMo4, starting at 850 °C: vcrit ≈ (850 − 500) / 10 = 35 °C/s
heart in oil: v ≈ (850 − 500) / 12 = 29.2 °C/s
29 °C/s is one-tenth of the value required for C45, but close to the value required for 42CrMo4

The core of C45 in oil hardens into fine perlite and bainite, not martensite. 42CrMo4, on the other hand, hardens almost completely at the core, and with agitated oil or a slightly smaller bar, it hardens completely. This is why critical shafts are made of alloy steel: not because it is harder, but because it hardens to great depth when using a milder medium, which causes less deformation and cracking.

22.6 Hardening Methods and Hardenability

The quenching medium is the fluid in which the workpiece is cooled. A more aggressive medium cools faster and provides greater hardening, but it increases stresses, deformation, and the risk of cracking. The choice is always a compromise: the mildest medium that can still exceed the steel’s critical cooling rate across the workpiece’s thickness is used.

HalfIndicative severity HWhat is it used for?
Saltwater or water with baking soda2-5unalloyed steels with simple geometries; highest risk of cracking
Water1-2unalloyed steels (C40, C45, C60), simple workpieces that are not too thin
Aqueous polymer solutions0,3-1,2A middle ground that can be adjusted based on concentration; they do not burn, and the oil is replaced frequently; widely used in induction hardening
Frying oil0,3-0,8quenched and tempered and case-hardened alloy steels (42CrMo4, 39NiCrMo3, 16MnCr5)
Melted salts (150–550 °C)variable"step" and bainitic hardening: the workpiece is held above Ms to stabilize the temperature, resulting in minimal deformation
Pressurized gas in vacuum furnaces0,1-0,4high-alloy tools and die steels (X40CrMoV5-1, X153CrMoV12), clean and polished workpieces free of oxide
Still air or forced airabout 0.02high-alloy self-hardening steels; normalizing

H is the “agitation” of the medium, compared to still water (H = 1). Approximate values (rounded): these values increase significantly if the medium is agitated or the workpiece is moving.

A phenomenon worth knowing: in the first moment, a film of steam forms around the hot workpiece, which insulates it and slows down the cooling process. This is why the workpiece moves in the bath (or the bath becomes agitated), and it must be immersed the right way: with the shafts vertical, never lying flat; otherwise, they cool unevenly and warp.

Hardenability and Jominy Test

We need to distinguish between two words that look the same:

  • Hardness refers to how hard the surface becomes; it depends on the carbon content (example 22.1);
  • Hardenability refers to the depth to which steel hardens; it depends primarily on the alloying elements and grain size.

Hardenability is measured using the Jominy test: a 100-mm-long, Ø25 cylindrical specimen, which has been austenitized, is suspended and quenched with a stream of water only on its underside. The wetted face cools very quickly, while the areas farther away cool at a gradually slower rate: a single specimen thus exhibits the full range of cooling rates. A strip is then planed along the specimen, and the HRC hardness is measured at increasing distances from the quenched face.

Ø25 test piece100 mm longmeasurement pointsalong one facewater jetfacehardened20304050601020304050042CrMo4 (highly hardenable)C45 (poorly hardenable)Hardness HRCDistance from the hardened surface (mm)
Figure 22.5 · On the left, the Jominy test; on the right, two schematic curves (indicative average values). C45 loses its hardness just a few millimeters from the hardened surface; 42CrMo4 remains hard at a much deeper depth.

The flatter the Jominy curve, the more hardenable the steel is. The initial hardness—that near the surface—depends on carbon content and is nearly the same for both steels; the subsequent decrease, however, depends on the alloy. The data sheets for steels with “guaranteed hardenability” (indicated by the letter H after the designation, for example, 42CrMo4+H) show a Jominy band, that is, the minimum and maximum permissible values.

💡
Mass effect. A large workpiece cools more slowly at its core than a small one, even in the same bath. For this reason, the strength values for quenched and tempered steel in the standards are given by diameter class: quenched and tempered C45, up to Ø16 mm, achieves much higher strengths than at Ø100. The values used in this manual (quenched and tempered C45 with Re approximately 490 N/mm² and Rm approximately 700 N/mm², quenched and tempered 42CrMo4 with Re approximately 750 N/mm² and Rm approximately 1000 N/mm², Chapter 10) apply to average diameters, around 40–100 mm.

22.7 Hardening, Tempering, and Annealing

Quenching is the heat treatment that transforms steel into austenite (Section 22.3) and cools it faster than the critical cooling rate (Section 22.5) to produce martensite. A freshly quenched workpiece is extremely hard but also as brittle as glass, and full of internal stresses: if left as is, it can crack on its own even after just a few hours. For this reason, quenching is always followed immediately by tempering.

Tempering involves heating below A1, usually between 150 and 700 °C, with a holding time of at least 1–2 hours, followed by cooling in air. The carbon trapped in the martensite is gradually released and forms tiny carbides: hardness decreases, toughness increases, and internal stresses are relieved. The higher the tempering temperature, the tougher the workpiece becomes and the less hard it is. There are two approaches:

  • Low tempering, 150–250 °C: removes stress and some brittleness, but leaves almost all of the hardness intact. It is used for tools, gauges, case-hardened workpieces, and raceways;
  • High-temperature tempering, 550–700 °C: The workpiece loses much of its hardness but becomes both strong and tough. The combination of quenching and high-temperature tempering is called case hardening and is the most commonly used heat treatment for machine components: shafts, connecting rods, high-strength screws, flanges, and lightly loaded gears.
202530354045505560100200300400500600700620 °C42CrMo4 (oil)C45 (water)Brittleness:to be avoidedhardeninghardenedHardness (HRC)tempering temperature (°C)
Figure 22.6 · Hardness after two hours of tempering for small, fully hardened specimens (rounded approximate values; points connected by line segments). The hatched area indicates the selection for Example 22.7.
Tempering Temperature (°C)tempered200300400500550600650700
Water-hardened C45 (HRC)5755504334(29,5)2521< 20
Oil-hardened 42CrMo4 (HRC)555350464137322722

Approximate, rounded values prepared for this manual, for small-diameter samples. The 29.5 in parentheses is an interpolated value. For large workpieces, which are not hardened all the way through, the hardness values are lower: refer to the manufacturer’s data sheets for design values.

The temperature between two points on the graph is calculated using linear interpolation—that is, by assuming that the curve between the two points is a straight line:

Tempering temperature for a specified hardness
T = T1 + (T2 − T1) · H1 − HH1 − H2
T = desired tempering temperature in °C · H = required hardness · T1, H1 and T2, H2 = the two points on the curve between which H lies (H1 is the highest hardness at the lowest temperature, T1)
Example 22.7 · Hardening of 42CrMo4 to 28–32 HRC

The drawing specifies “Bonificato 28-32 HRC” for a 42CrMo4 shaft that is small enough to be fully hardened. At what temperature should it be tempered?

The target is the midpoint of the range: H = (28 + 32) / 2 = 30 HRC
30 falls between 600 °C (32 HRC) and 650 °C (27 HRC)
T = 600 + (650 − 600) · 32 − 3032 − 27 = 600 + 50 · 0,4 = 620 °C
Hardness test: 30 HRC ≈ 286 HB, Rm ≈ 3.4 × 286 = 972 N/mm²
Melting point at approximately 620 °C; tensile strength around 1000 N/mm², as specified in Chapter 10

The conversion between hardness values and the approximate relationship Rm ≈ 3.4 · HB for steels can be found in Chapter 19. In practice, the heat treatment operator performs tempering, measures the hardness, and, if the workpiece is still too hard, tempers it again at a slightly higher temperature: tempering can be repeated, but incorrect hardening cannot.

Example 22.8 · A C45 pin with a hardness of 40 HRC

A water-hardened C45 pin should have a hardness of approximately 40 HRC. What type of tempering is required?

40 falls between 400 °C (43 HRC) and 500 °C (34 HRC)
T = 400 + (500 − 400) · 43 − 4043 − 34 = 400 + 100 · 0,333 = 433,3 °C
Melting point at approximately 430 °C

Two notes on tempering. First: certain steels, when tempered between approximately 250 and 350 °C, become more brittle rather than more tough (this is known as temper brittleness); that range, marked in red in Figure 22.6, should be avoided when seeking toughness. Some nickel-chromium steels have a second dangerous range around 450–550 °C, which molybdenum mitigates: this is why 42CrMo4 and 39NiCrMo3 are so widely used. Second: tempering must be performed immediately after quenching, on the same day, and preferably while the workpiece is still lukewarm.

Tempering Colors

A clean, polished steel surface, heated in the open air, becomes covered with an increasingly thick layer of oxide, which changes color with temperature due to light interference. Blacksmiths used to temper their chisels by observing their colors; today, these colors are still used to identify an overheated workpiece during grinding (burn marks exhibit precisely these colors).

ColorApproximate temperature (°C)Traditional Use
light straw yellow200-220cutting tools, calipers
dark straw yellow230-240punches, marking points
brown, reddish-brown250-270chisels, dies
purple, violet280-290woodworking tools, axes
blue300-320springs, screwdrivers
blue-graymore than 330no longer legible

Approximate values: The color also depends on the holding time and the type of steel, and above 330 °C, it is no longer indicative.

22.8 Annealing and Normalizing

Annealing is the opposite of hardening: the material is heated and cooled slowly, usually in a turned-off furnace, to achieve a soft, uniform structure free of stress. These treatments are often performed before machining operations or between machining operations, and the end customer hardly ever notices them.

  • Full annealing: As with quenching, to A3 + 30–50 °C in hypoeutectoid steels, followed by very slow cooling in the furnace. This produces coarse pearlite and ferrite: the softest and most ductile steel possible. It is used to eliminate the effects of previous machining operations or improper hardening.
  • Workability or globulization annealing (also called “softening” annealing): a long hold at a temperature just below A1, around 680–720 °C, or fluctuating around A1 for hypereutectoid steels. The lamellar cementite aggregates into small globules: the steel becomes softer, chips break more easily, and tools last longer. This is essential for high-carbon steels (100Cr6, tool steels) before turning or milling them, and for steels intended for cold forming.
  • Stress-relief annealing: at 550–650 °C, below A1, with slow cooling. It does not change the microstructure but removes internal stresses after welding, straightening, and heavy roughing. For a workpiece that has already been heat-treated, this is performed at a temperature at least 30–50 °C below the tempering temperature, so as not to reduce its hardness.
  • Normalizing: The metal is heated to a slightly higher temperature than for quenching, approximately A3 + 50–80 °C, and allowed to cool in still air. The grain becomes fine and uniform, and the structure consists of fine pearlite with ferrite: strength is slightly higher than after annealing, with good toughness. It is used on forged, rolled, and welded workpieces, and as a preparation for hardening. Steels sold as “normalized” include the letter N in their designation (Chapter 20).
6007008009001,00050000.20.40.60.81.01.2A3AcmA1 · 727 °Cglobularizationrelaxationnormalizinghardening and full annealingtemperature (°C)carbon (% by mass)
Figure 22.7 · Heat treatment temperatures on the simplified iron-carbon diagram (indicative ranges). Quenching and full annealing use the same range; the only difference is the cooling rate—rapid for quenching and very slow for annealing.
🛠️
In the workshop. A round bar of quenched-and-tempered steel usually arrives already quenched and tempered (marked +QT) or annealed (+A). If a lot of turning is required and the workpiece will be hardened anyway, it’s best to buy it annealed, as it’s easier to machine; if the finished part must remain quenched and tempered, buy it in that condition and machine it directly, accepting that the machining will be more difficult.

22.9 Induction and Flame Surface Hardening

Often, it’s enough for just the surface to be hard: the seat of a pin, the teeth of a gear, or the sealing area of a shaft. With surface hardening, only the outer layer above A3 is heated—very quickly—and then immediately cooled with a spray of water or polymer. The core remains as it was, usually case-hardened and therefore tough. The steel must contain enough carbon to harden on its own: typical grades include C45, 42CrMo4, 41Cr4, and C53.

  • Induction: A copper coil through which high-frequency alternating current flows (the inductor) creates a magnetic field that induces electric currents in the surface of the workpiece. These currents heat the metal in a matter of seconds. The higher the frequency, the more the currents remain on the surface and the thinner the hardened layer. This method is used for large production runs; it is clean and repeatable, and the inductor is shaped to fit the workpiece.
  • Flame: An oxyacetylene torch heats the surface, followed by a water spray. Deeper layers; simple equipment, suitable for large, individual workpieces (pallet rails, large gear wheels), but less precise.
copper inductorshowertempered glassThe inductor moves to the right; the shower follows30040050060012340440 HV = 0.8 × 550Rht ≈ 2 mmhardened coreHV hardnessDepth (mm)
Figure 22.8 · On the left, “step-by-step” induction hardening: the inductor moves along the shaft, and the cooling spray immediately cools the heated area. On the right, the hardness profile (schematic) and the hardening depth Rht, measured where the hardness drops to 80% of the minimum required hardness at the surface.

The thickness through which almost all of the current flows is called the penetration depth, and for steel that is already hot (above the temperature at which it ceases to be magnetic, approximately 770 °C), it is estimated as follows:

Current Penetration Depth (Hot-Rolled Steel, Overview)
δ ≈ 500√f
δ penetration depth in mm · f current frequency in Hz. Simplified and approximate formula: the actual hardened layer also depends on the power and heating time, and is usually slightly less than δ.
Example 22.9 · What is the frequency for 2 mm?

We want to induction-harden a C45 pin to a depth of about 2 mm. What frequency is needed? And what depths would 10 kHz and 100 kHz produce?

from the formula: √f = 500 / δ → f = (500 / δ)² = (500 / 2)² = 250² = 62,500 Hz
at 10 kHz: δ ≈ 500 / √10,000 = 500 / 100 = 5.0 mm
at 100 kHz: δ ≈ 500 / √100,000 = 500 / 316.2 = 1.58 mm
A frequency in the range of 50–100 kHz is required

Low frequencies (1–10 kHz) are used for deep layers and large workpieces, while high frequencies (100–450 kHz) are used for thin layers, small teeth, and minute workpieces. After induction hardening, a low-temperature tempering treatment is performed, often using the same inductor or in an oven at 150–200 °C. Typical hardness values: 55–60 HRC for C45 and 42CrMo4.

22.10 Case Hardening

Low-carbon steels (0.1–0.25%) do not harden, but they are very tough. Case hardening makes them suitable for gear wheels, chain pins, and splined shafts: the surface layer is enriched with carbon, up to about 0.7–0.9%, and then hardened. This produces an extremely hard surface (58–62 HRC) over a tough core (30–45 HRC). It is a thermochemical treatment: it changes the composition of the surface, not just its structure.

  • Carburizing: The workpiece is held for hours at 900–950 °C, in the austenitic phase, in a carbon-rich atmosphere (endothermic gas mixed with methane or propane; historically, coal dust or salts). Carbon enters the surface and diffuses inward; modern low-pressure furnaces use acetylene;
  • hardening, in oil or gas, either directly from the carburizing temperature or after lowering it to approximately 820–860 °C;
  • Low-temperature tempering at 150–200 °C, to relieve stress while maintaining hardness.

The most common case-hardening steels are C10 and C15 (small, lightly loaded workpieces), 16MnCr5 and 20MnCr5 (gears and transmission shafts), and 18CrNiMo7-6 (highly loaded gears, large thicknesses). Areas that must not be hardened—for example, threads to be machined later—are protected with special paints or with an allowance that is removed before hardening.

4005006007008000.20.40.60.80.51.01.52.02.50Eht = 1.0 mm550 HVHardness (HV)carbon (%)core: 0.2% CHV% CDepth from the surface (mm)
Figure 22.9 · Schematic profile after carburizing, quenching, and low-temperature tempering of a 16MnCr5 steel: the carbon content (light blue hatching, right scale) decreases from 0.8% at the surface to 0.2% at the core; hardness (red, scale on the left) follows suit. The effective depth Eht is measured where the hardness drops to 550 HV.

The thickness of the case-hardened layer is indicated by the effective case-hardening depth, Eht (referred to as CHD, or case hardening depth, in recent ISO standards): it is the distance from the surface at which the hardness drops to 550 HV. It is measured on a cross-sectioned specimen using a series of Vickers indentations. Typical values range from 0.3 mm for small workpieces up to 2 mm or more for large gears; a rule of thumb used by gear designers specifies an Eht of approximately 0.15–0.2 times the module.

Carbon spreads like an inkblot on paper: at first it travels, then it slows down. The depth increases as the square root of time:

Depth of Hardening and Time (Law of the Square Root of Time)
x = K · √t , so t = x²K²
x effective depth in mm · t carburization time in hours · K constant that depends on temperature, atmosphere, and steel: at 920–930 °C, the effective depth is approximately 0.5 mm/√h. The actual value is provided by the heat treatment specialist for their specific furnace.
Example 22.10 · How long does the cementation process last?

A 16MnCr5 wheel must have “Eht 0.8–1.2.” Given K = 0.5 mm/√h, how long must the carburizing process last to fall within the middle of the range? And for the two extremes?

center: x = (0.8 + 1.2) / 2 = 1.0 mm → t = 1.0² / 0.5² = 1 / 0.25 = 4.0 h
minimum: t = 0.8² / 0.25 = 0.64 / 0.25 = 2.56 h
maximum: t = 1.2² / 0.25 = 1.44 / 0.25 = 5.76 h
About 4 hours of carburization; the tolerance ranges from about 2½ hours to nearly 6 hours

Doubling the depth means quadrupling the time: a 2-mm layer would require 2² / 0.25 = 16 hours. This is one of the reasons why deep case-hardened workpieces are so expensive.

⚠️
Case-hardened also means deformed. Case hardening is performed at 900–950 °C, the highest temperature among common heat treatments, and is followed by quenching: the workpieces deform and increase in size. Case-hardened gears are ground or polished on the teeth, the holes are reamed, and the bearing seats are ground. See section 22.14.

22.11 Nitriding and Carbonitriding

Nitriding involves introducing nitrogen into the surface of the steel at a low temperature, between approximately 500 and 570 °C. The nitrogen bonds with the iron and, above all, with the alloying elements (aluminum, chromium, molybdenum, vanadium), forming extremely fine and extremely hard nitrides. No subsequent hardening is required: the hardness is achieved right away.

  • Very high hardness: approximately 600–800 HV for chromium-molybdenum steels (31CrMoV9, 42CrMo4), and 900–1,100 HV on specially formulated chromium-aluminum steels (34CrAlMo5, 41CrAlMo7). The hardness is maintained even if the workpiece is heated to approximately 500 °C;
  • almost no deformation: the temperature is lower than the tempering temperature, and there is no hardening, so the core structure does not change. The workpiece expands by only a few centimeters due to the nitrogen that is introduced. A finished part can be nitrided;
  • thin layers: 0.1 to 0.6 mm of diffusion, plus a hard surface layer of compounds (the “white layer”) measuring 5–20 µm, which is highly resistant to wear and corrosion but may flake off under impact loads;
  • Long processing times: 20 to 80 hours in gas nitriding.

Before nitriding, the workpiece must be heat-treated (the core must be able to support the hardened layer) at a temperature higher than the nitriding temperature, and must already have been finished. The following types are distinguished:

  • gas nitriding, in an ammonia furnace at 500–530 °C: simple, suitable for large loads;
  • ion nitriding (or plasma nitriding): the workpieces are placed in a low-pressure chamber containing nitrogen and hydrogen, and an electric current creates a plasma that bombards the surface. Shorter processing times, precise control of the white layer, and easy protection of areas to be left unnitrided using metal plates;
  • nitrocarburizing (ferritic, at approximately 570–580 °C, in gas or in salts, also known by trade names): nitrogen and a small amount of carbon; takes a few hours; produces a thin layer that is highly resistant to wear and seizing; used on shafts, pins, and weapon parts, often followed by black oxidation.

Here, too, the depth increases with the square root of time, but much more slowly than in cementation, because the temperature is low.

Example 22.11 · How long does nitriding take?

Gas nitriding results in a depth of 0.4 mm in 50 hours. What is the value of the constant K? How long would it take to achieve a depth of 0.3 mm?

K = x / √t = 0.4 / √50 = 0.4 / 7.071 = 0.0566 mm/√h ≈ 0.057
t = 0,3² / 0,057² = 0,09 / 0,003249 = 27,7 h
K ≈ 0.057 mm/√h · approximately 28 hours for 0.3 mm

With a carburization factor of K = 0.5, 0.3 mm would take 0.36 hours. The long processing time is the price to pay for avoiding deformation.

Carbonitriding, on the other hand, is a variation of case hardening: carbon and a small amount of nitrogen are introduced at 820–880 °C, followed by quenching in oil and low-temperature tempering. Nitrogen increases the hardenability of the surface layer, so a gentler quenching process is sufficient and the temperature can be lower: this results in less distortion than case hardening and allows for thinner surface layers (0.1–0.7 mm). It is suitable for small workpieces made of non-alloy steel: self-tapping screws, small gears, and pins.

22.12 Non-thermal coatings and surface treatments

Many workpieces undergo a surface treatment that does not involve a furnace: a coating of another metal, an oxide layer, or a ceramic coating. These are used to protect against corrosion, wear, and seizing, or for aesthetic purposes. They share one important characteristic for those who work with machines: they add thickness, and dimensions must be calculated accordingly.

1 µm10 µm0.1 mm1 mm10 mmblackeningPVD (TiN, TiAlN)CVD (inserts)electrolytic zinc platingChemical nickel platinganodizinghard chrome platingshot peening (compressed layer)nitridingcarbonitridingcase hardeninginduction hardeningflame hardening
Figure 22.10 · Typical thicknesses or depths of treatments, on a logarithmic scale (approximate values). Yellow indicates overcoats, light blue indicates ceramic coatings, red indicates thermal and thermochemical treatments, and green indicates shot peening.

Electroplated Coatings

In the electroplated overlays (or electrolytic plating) the workpiece is immersed in a bath containing the salts of the metal to be deposited and is connected to the negative terminal: the current deposits the metal onto the surface, atom by atom.

  • Electrolytic galvanizing, 5–25 µm: protects steel from rust even if scratched, because the zinc corrodes instead of the iron. The process is completed with a passivation treatment (nowadays based on trivalent chromium, which is iridescent, black, or transparent). For outdoor structures, hot-dip galvanizing—where the steel is immersed in molten zinc—is used, resulting in a much thicker coating (50–150 µm). Caution regarding high-strength bolts (class 10.9 and above): the hydrogen in the bath can embrittle them; they must be “dehydrogenated” in an oven at approximately 200 °C immediately after treatment;
  • Hard chrome plating, ranging from 10 µm to a few tenths of a millimeter: an extremely hard layer of chromium (800–1000 HV) with low friction, used for hydraulic cylinder rods, rollers, and pins. It is deposited thicker than necessary and then ground down. Baths containing hexavalent chromium are subject to increasingly stringent environmental regulations, and alternatives are being sought;
  • Nickel plating: Electrolytic nickel plating is decorative and provides corrosion protection; chemical nickel plating (nickel-phosphorus, currentless) deposits a uniform layer even inside holes and on edges, 5–50 µm, with a hardness of approximately 500–600 HV, increasing to about 900–1,000 HV after heating to approximately 400 °C. Excellent for molds and precision parts.
Example 22.12 · Dimensions of a stem before chrome plating

A stem must have a finished diameter of 30 and be chrome-plated. The final chrome plating must be 0.03 mm thick on each side; the chrome plater deposits 0.06 mm on each side, and then it is ground down. To what diameter is the base material ground before chrome plating? How much material is removed during the final grinding?

base diameter = 30 − 2 × 0.03 = 29.94 mm
after chrome plating: 29.94 + 2 × 0.06 = 30.06 mm
Final grinding: 30.06 − 30 = 0.06 mm on the diameter (0.03 per side)
Base ground to Ø29.94; after chrome plating, Ø30.06; final grinding of 0.06 mm on the diameter

Burnishing

Burnishing (or black oxidation) is a hot alkaline bath, at around 140 °C, that transforms the surface into a thin black layer of iron oxide, approximately 1 µm thick. It does not alter dimensions, is economical and elegant, but offers little protection against rust: it must always be followed by a coat of oil or wax. It is used for equipment, screws, machine parts, and weapons.

Aluminum Anodizing

Anodizing causes a layer of aluminum oxide to form on the surface of the aluminum by connecting the workpiece to the positive terminal in an acidic bath (Chapter 21). The oxide is hard, insulating, and corrosion-resistant, and it can be colored. The typical layer thickness is 5–25 µm; hard anodizing at low temperatures can reach 25–100 µm with hardnesses of 400–500 HV. Unlike electroplated coatings, the layer is formed by transforming the metal itself: approximately half of its thickness grows outward and half inward.

Diameter Variation Due to Anodizing
ΔD ≈ 2 · s2 = s
ΔD: increase in the diameter of a pin (decrease for a hole) in µm · s; total thickness of the anodic layer in µm. Half the thickness, on two opposite sides.
Example 22.13 · A hard-anodized aluminum pin

An aluminum alloy pin must measure Ø20 after a 40 µm hard anodizing process. To what diameter should it be turned? And for a Ø20 hole, what size should it be?

ΔD ≈ 40 µm = 0.04 mm
pin: turn to 20 − 0.04 = 19.96 mm
hole: the dimension is 20 + 0.04 = 20.04 mm
Pin Ø19.96 and hole Ø20.04 before anodizing

PVD and CVD Coatings

Thin ceramic coatings are deposited in vacuum chambers.

  • PVD (physical vapor deposition), at 200–500 °C: a metal (titanium, aluminum, chromium) is vaporized and reacts with the nitrogen in the chamber, depositing a layer 1–5 µm thick. The best-known coatings are TiN (titanium nitride, gold-colored, approximately 2300 HV) and TiAlN (titanium aluminum nitride, purplish-gray, approximately 3000–3300 HV, with better heat resistance). The low temperature allows even hardened steel tools and dies to be coated without softening them;
  • CVD (chemical vapor deposition), at 900–1050 °C: gases react on the surface and form layers 5–20 µm thick, such as titanium carbonitride and aluminum oxide. High temperatures are suitable for cemented carbide inserts, but not for hardened steels, which would lose their hardness.

These are the coatings used on cutting tools: inserts, end mills, and drill bits. Their characteristics and the appropriate selection for each material are covered in Chapter 25. Amorphous carbon (DLC) coatings, which have extremely low friction, are also used on workpieces.

22.13 Shot peening and rolling

Most fatigue fractures (Chapter 10) originate at the surface, where bending and torsional stresses are greatest and where there are machining marks, scratches, and notches. A crack will form only if it is under tension; if the surface is under compression, the crack has difficulty initiating and propagating. Shot peening and roller burnishing serve precisely this purpose: they cold-deform a thin layer and leave it with residual compressive stresses.

  • shot peening (shot peening): The surface is struck by a stream of small steel, glass, or ceramic balls. Each ball leaves a tiny indentation and stretches the metal beneath it; the surface layer, which would expand but is held back by the core, remains compressed. It is used on springs, gears, connecting rods, blades, and shaft fillets. It is checked using test gauges (Almen) and by measuring the coverage;
  • Rolling: A hard roller, driven with force, passes over the surface of a fillet, a groove, or a track. In addition to compressing the layer, it flattens the peaks of the roughness and polishes the surface. Rolled threads, which are cold-formed rather than cut, have continuous material fibers and a compressed base: they resist fatigue much better than cut threads (Chapter 23).
2000−200−400−600−8000.10.20.30.40.50.6Compression: prevents cracksslight tensile stress at the coreResidual stress (N/mm²)depth (mm)
Figure 22.11 · Schematic residual stresses after shot peening: the surface layer, up to about 0.3 mm, remains under compression; beneath it, for the sake of equilibrium, there is a small tensile stress.
Example 22.14 · How much does shot peening cost?

A heat-treated C45 steel shaft has an Rm of 700 N/mm². The fatigue limit of a smooth specimen under rotational bending is approximately half of Rm (Chapter 10). If proper shot peening increases it by 25% (as a rough guide: the increase ranges from 10–20% on smooth workpieces to over 50% on notched workpieces), what will the value be?

σf ≈ 0.5 × 700 = 350 N/mm²
after shot peening: 350 × 1.25 = 437.5 N/mm²
From approximately 350 to approximately 440 N/mm²: the same shaft can withstand higher alternating loads without changing the steel grade or dimensions

Residual stresses are eliminated if the workpiece gets too hot; this is why shot peening is performed after hardening and tempering, and the compressed layer is not ground away.

22.14 Deformations, Drawing Specifications, and Machining Cycle

The workpiece changes in size and shape

Any heat treatment process slightly alters the dimensions of the workpiece. There are two reasons for this:

  • volume change: martensite occupies more space than the pearlite and ferrite from which it forms, so a thoroughly hardened workpiece usually expands—roughly by about 0.1% in linear dimensions for a quenched-and-tempered steel (this depends on the steel, shape, and heat treatment: it may also shrink);
  • Deformations: The surface and the core cool at different rates—the thin parts before the thick ones—creating stresses that warp the workpiece. Long shafts bend, rings become oval-shaped, and plates warp. Residual stresses from previous machining operations also play a role, and the furnace “releases” them.

To minimize the problem: design workpieces that are symmetrical and have uniform thicknesses, with fillets and no sharp edges (which are also the points where hardening cracks form); stress relief is performed after heavy roughing; a alloy steel that hardens to a soft temper is selected; the workpiece is immersed in the correct orientation. And allow for an allowance for finishing after the heat treatment, using a grinding wheel or CBN tools (Chapters 25 and 29).

Allows for grinding after hardening on the diameter
s = 2 · (e + amin ) ΔL ≈ εt · L
s allowance to be left on the diameter in mm · e Maximum radial runout after treatment and straightening (half the runout reading on the dial gauge) in mm · amin Minimum removal per side, to remove the decarburized layer and obtain a clean surface, usually 0.05–0.1 mm · ΔL Change in dimension L for the treatment · εt relative change, approximately 0.001 (i.e., 0.1%) for full hardening
Example 22.15 · Allowance for a Ø40 h6 shaft

A 300 mm long 42CrMo4 shaft must be ground to Ø40 h6 after hardening and tempering. Experience shows that, after straightening, it shows a runout of 0.12 mm on the dial indicator; the goal is to remove at least 0.1 mm per side. What allowance should be made on the lathe? What will actually be removed during grinding?

e = 0.12 / 2 = 0.06 mm
s = 2 · (0.06 + 0.1) = 2 · 0.16 = 0.32 mm → turn to Ø40.35 (rounding up)
Increase in diameter: ΔD ≈ 0.001 × 40 = 0.04 mm → approximately Ø40.39 after treatment
Increase in length: ΔL ≈ 0.001 × 300 = 0.3 mm
During grinding, 40.39 − 40 = 0.39 mm is removed from the diameter
Turn to Ø40.35; approximately 0.4 mm will be removed from the diameter during grinding. The length may increase by approximately 0.3 mm: tight length dimensions are finished after heat treatment

If the allowance is too thin, it leaves black (unground) or soft (decarburized) areas; if it is too thick, it wastes time and, if ground aggressively, risks causing burn marks and grinding cracks. In case-hardened workpieces, the allowance is removed from the hardened layer, so it must be added to the required Eht: the person performing the case hardening must know how much will be removed later.

How to Write a Custom Treatment with a Drawing

Heat treatment is as much a part of the workpiece as dimensions and tolerances, and must be specified on the drawing, usually near the title block or with a note and a reference to the relevant area (the applicable standard is ISO 15787). The specification must state what it's done, as a result desired, measurable, and where. Temperatures and times are not recorded—those are the heat treatment specialist’s responsibility—but hardness values and depths, along with their tolerances, are recorded.

Drawing NoteWhat does that mean?
Hardened to 28–32 HRChigh-temperature quenching and tempering; surface hardness measured between 28 and 32 HRC
Hardened and tempered to 54–58 HRChardening with low tempering; the workpiece is hard throughout its entire cross-section
Case-hardened and tempered to 58–62 HRC, Eht 0.8–1.2Surface hardness 58–62 HRC; at 550 HV, the depth must be between 0.8 and 1.2 mm
Induction-hardened to 55–60 HRC, Rht 1.5–2.5 (area indicated by a thick dashed line)only the marked area; Rht is the depth at which the hardness drops to 80% of the surface minimum (now SHD)
Nitrided to 700 HV1 min, Nht 0.3–0.5Vickers hardness with a load of 1 kgf; Nht is the depth at which the hardness exceeds that of the core by 50 HV (now NHD)
Annealed to a maximum of 220 HBsoftened material for machining operations
Fe/Zn 8 galvanized, trivalent passivation8 µm electrolytic zinc plating on steel, with passivation

The areas to be treated or protected are marked on the drawing with a thick dashed line parallel to the outline, with the length dimensioned (Chapter 11). It is good practice to also indicate where to measure the hardness if the surface is not uniform throughout.

The machining cycle of a processed workpiece

Steel hardened to 58 HRC can no longer be machined with standard tools. For this reason, the machining process for a heat-treated workpiece is always divided into three stages:

  • machining of soft material (annealed or tempered): turning, milling, drilling, and threading, with an allowance on the surfaces that will be finished later. Threaded holes and small parts are finished at this stage, because it would no longer be possible to do so later;
  • heat treatment, with stress relief if necessary beforehand, followed by straightening and inspection (hardness, depth on a sample, deflection);
  • Hard-surface finishing: grinding, hard turning with CBN inserts, polishing, electrical discharge machining. Only functional surfaces are finished: bearing seats, raceways, and centering surfaces.
BlankØ45 barRoughingturned toØ40.35Hardening andtemperingØ40.39Straighteningand inspectiondeflectionGrindingØ40 h6InspectionAllowance left on the lathe: 0.35 mm on the diameterAll of this is removed during grinding, along with the growth layer and the decarburized layerSoft: machined with standard toolsHard: grinding wheel or CBN only
Figure 22.12 · The machining sequence for the shaft in Example 22.15: rough machining with an allowance, heat treatment, inspection, and grinding to the final dimension.
🖥️
Try it in CNC Code. In the lathe simulator, enter the roughing program for the shaft using the dimension Ø40.35 instead of Ø40: this is the “work-in-progress” version of the workpiece. That way, you can immediately see where an allowance is needed and where the dimension is already finished.

10:15 p.m. The formulas in this chapter

What Are You Looking For?FormulaUnits
Maximum hardness of martensite (C ≤ 0.5%)HRCmax ≈ 20 + 60 · √CHRC
Line A3 of the simplified diagramA3 ≈ 912 − 211 · √C°C
Hardening of hypoeutectoid steelsT = A3 + 30 ÷ 50°C
Hardening of Hypereutectoid SteelsT = 727 + 30 ÷ 50°C
Baking time (approximate)t ≈ k · s (k = 1 for unbound, 1.5 for bound)min
Heat to warm the loadQ = m · c · ΔT / 3600kWh
Oven Cycle EnergyE = Q / η + Pd · tpkWh
Average cooling ratev = (T1 − T2) / Δt°C/s
Tempering temperature (interpolation)T = T1 + (T2 − T1) · (H1 − H) / (H1 − H2)°C
Induction Depth of Penetrationδ ≈ 500 / √fmm
Hardening or Nitriding Depthx = K · √t · t = x² / K²mm · h
Increase in Diameter Due to AnodizingΔD ≈ sµm
Grinding Allowances = 2 · (e + amin)mm
Dimensional change due to heat treatmentΔL ≈ εt · L (where εt is approximately 0.001)mm

Formulas using “≈” and the constants k, K, c, and εt are guidelines for understanding orders of magnitude and performing initial calculations. The actual values for a specific workpiece are provided in the steel data sheets and by the heat treatment specialist.

22.16 Exercises

Use the example values from the chapter. Try to solve them on your own, using a calculator, before looking at the solution.

Exercise 1. Using the formula from the simplified diagram, find line A3 and the quenching temperature for C35 (0.35% C).
Solution

A3 ≈ 912 − 211 · √0.35 = 912 − 211 · 0.5916 = 912 − 124.8 = 787.2 °C. Quenching: from 787.2 + 30 = 817.2 to 787.2 + 50 = 837.2 °C, approximately 820–840 °C.

Exercise 2. A tool steel contains 1.2% carbon. At what temperature is it hardened? Why isn’t it heated above the Acm line, which, in the simplified diagram, corresponds to approximately 862 °C at 1.2% C?
Solution

It is hypereutectoid: T = 727 + 30 ÷ 50 = 757–777 °C. Above Acm (727 + 314 × 0.43 = 862 °C), all the cementite would dissolve: the grain size would increase, the workpiece would become more brittle, and a significant amount of austenite would remain untransformed after quenching. The undissolved carbides, on the other hand, increase wear resistance.

Exercise 3. What is the maximum hardness of martensite in 42CrMo4 (0.42% C)? How does this differ from C45?
Solution

HRC ≈ 20 + 60 · √0.42 = 20 + 60 · 0.6481 = 58.9 HRC, roughly the same as C45 (60.2). Hardness depends on carbon content; the difference lies in hardenability: 42CrMo4 achieves that hardness even at the core of larger workpieces and using a milder quenching medium (oil).

Exercise 4. A 30-mm-thick 42CrMo4 plate and an 80-mm-diameter C45 round bar are to be hardened. Using the rule of thumb, how long should they remain at that temperature?
Solution

Sheet: t ≈ 1.5 × 30 = 45 min. Round: t ≈ 1 × 80 = 80 min. Both are above the minimum of 20 minutes; the times are counted from when the oven has reached the desired temperature again.

Exercise 5. An electric furnace heats 150 kg of workpieces from 20 to 860 °C, with c = 0.6 kJ/(kg·K) and an efficiency of 0.5. During the 1.5-hour holding period, it loses 6 kW. With electricity costing 0.22 €/kWh, how much does the cycle cost?
Solution

Q = 150 · 0.6 · 840 / 3,600 = 75,600 / 3,600 = 21.0 kWh; E = 21.0 / 0.5 + 6 × 1.5 = 42.0 + 9.0 = 51.0 kWh; cost = 51.0 × 0.22 = 11.22 €.

Exercise 6. Using the table in paragraph 22.7, at what temperature should a C45 steel, quenched in water, be held to achieve a hardness of 45 HRC? And what about a 42CrMo4 steel for 37 HRC and 35 HRC?
Solution

C45: between 300 °C (50) and 400 °C (43): T = 300 + 100 · (50 − 45) / (50 − 43) = 300 + 71.4 = 371.4 °C, approximately 370 °C (outside the 250–350 range to be avoided). 42CrMo4 at 37 HRC: this is a specific point in the table, 550 °C. At 35 HRC: between 550 (37) and 600 (32): T = 550 + 50 · 2/5 = 570 °C.

Exercise 7. A deep induction hardening depth of approximately 1.5 mm is desired. What frequency does the penetration depth formula indicate?
Solution

f = (500 / 1.5)² = 111,111 Hz, or about 100 kHz.

Exercise 8. Given K = 0.5 mm/√h, how long must the carburizing process last to achieve Eht = 0.6 mm? And for 1.5 mm? What depth is achieved in 6 hours?
Solution

0.6 mm: t = 0.36 / 0.25 = 1.44 h (about 1 hour and 26 minutes). 1.5 mm: t = 2.25 / 0.25 = 9.0 h. In 6 hours: x = 0.5 · √6 = 0.5 · 2.449 = 1.22 mm.

Exercise 9. Using the constant K = 0.057 mm/√h from Example 22.11, what is the nitriding depth achieved in 60 hours?
Solution

x = 0.057 · √60 = 0.057 · 7.746 = 0.44 mm.

Exercise 10. A Ø25 pin must be ground after hardening. After heat treatment, it shows a runout of 0.08 mm on the dial indicator, and at least 0.08 mm needs to be removed from each side. What diameter is left on the lathe? If the diameter increases by 0.1%, how much will be removed during grinding?
Solution

e = 0.08 / 2 = 0.04 mm; s = 2 · (0.04 + 0.08) = 0.24 mm: turn to Ø25.24. Expansion: 0.001 × 25 = 0.025 mm, so after heat treatment, the diameter is approximately Ø25.265; during grinding, approximately 0.265 mm is removed from the diameter.

Exercise 11. A hole in an aluminum plate must measure Ø12 after anodizing to a thickness of 20 µm. To what size is the hole reamed before the treatment?
Solution

ΔD ≈ s = 20 µm = 0.02 mm, and for a hole, the diameter decreases: it is reamed to 12 + 0.02 = 12.02 mm.

Exercise 12. A quenched and tempered 42CrMo4 shaft has an Rm of 1000 N/mm². Estimate the fatigue strength of the smooth specimen and the value after roll forming the fillet, which increases it by 30% (approximate value).
Solution

σf ≈ 0.5 × 1000 = 500 N/mm²; after rolling, 500 × 1.3 = 650 N/mm².

Exercise 13. A 20MnCr5 gear must have hardened teeth and a tough core, with any deformations to be corrected afterward. A finished 31CrMoV9 pin must be surface-hardened without deforming. A 2-meter-long pallet guide made of C45 steel must be hardened only on the raceway. Which heat treatment would you choose for each part, and how would you specify it on the drawing?
Solution

Wheel: case hardening, quenching, and low-temperature tempering, for example, “Case-hardened and quenched to 58–62 HRC, Eht 0.8–1.2,” followed by tooth grinding. Pin: nitriding, for example, “Nitrided 700 HV1 min, Nht 0.3–0.5,” performed on the finished part after heat treatment. Guide: Surface hardening by flame or induction of the raceway only, marked with a thick mixed line, for example, “Induction-hardened 52–56 HRC, Rht 2–3.”