Chapter 23

Non-removal machining operations

Not all workpieces are made from a bar of material that a lathe or milling machine shaves down into chips. Many are cast in a mold, hot-pressed between two dies, drawn into wire, cut and bent from sheet metal, pressed from powder, or built up layer by layer. These are non-material removal machining operations: they almost always prepare the blank that is then sent to the machine tools. In this chapter, we’ll look at how these processes work, what each one can achieve, and the calculations needed in the workshop: the dimensions of a foundry mold, the force of a press, the developed area of a bent sheet of metal, and the disc for a deep-drawn glass.

23.1 How to Shape a Workpiece

There are a few basic ways to shape a workpiece of metal into a specific form:

  • casting: the metal is melted and poured into a mold shaped like the final workpiece (foundry);
  • deforming it: taking solid metal and forcing it to change shape without breaking it, either while hot or cold (forging, rolling, extrusion, sheet metal machining);
  • removing material from a larger blank: using a tool that chips away material (turning, milling, grinding, as described in Chapter 24) or using the energy of a laser beam, an electric arc, or a water jet (non-conventional machining operations);
  • adding material: compacting and sintering a powder, or building the workpiece layer by layer (additive manufacturing);
  • Join multiple pre-made parts: screws, pins, and soldered joints (Chapter 18).
Metal machining operationsMachiningchip machiningNon-material removalturningmillingdrillinggrinding(Chapters 24–30)FoundrysandshellDie-castinglost-waxcentrifugal castingDeformationplasticforgingstampingrollingextrusiondrawingSheet metalblankingpunchingBendingDeep drawingcalenderingMetallurgypowder metallurgypressingsinteringcalibrationNon-conventionallaserplasmaoxy-fuel cuttingwaterjetelectrical discharge machiningManufacturingAdditiveFDMSLASLSlaser meltingJoining workpieces by welding is covered in Chapter 18
Figure 23.1 · Machining operations. This chapter covers the right-hand branch; unconventional machining operations remove material, but without a tool that cuts chips.

Non-machining operations have two major advantages: they waste no material (or very little) and are extremely fast in mass production—a press cuts a workpiece in a fraction of a second, and a die-casting mold produces one casting per minute. On the other hand, they require expensive equipment (molds, dies, and templates) and cannot, on their own, achieve tight tolerances. For this reason, the typical manufacturing process for a mechanical workpiece is as follows: the blank is produced by casting, forming, or cutting, and then only the surfaces that must be precise are finished with machine tools.

ProcessWhen It's Worth ItExamples of workpieces
FoundryComplex, hollow shapes, even very large ones; materials that do not deform well (cast iron)machine bases, pump housings, engine heads, crankcases
Forging and Stampingworkpieces subject to high stress, which must withstand impacts and fatigueshafts, connecting rods, keys, flanges, hooks
Rolling, extrusion, drawinglong semi-finished products with a constant cross-sectionsheet metal, beams, bars, tubes, structural sections, files
Sheet metal (cutting, bending, deep drawing)thin, lightweight workpieces, mass-producedbrackets, car bodies, electrical cabinets, cans, pots and pans
SinteringSmall workpieces produced in very large quantities, with a finished shapepump gears, self-lubricating bushings, pawls
Laser, plasma, waterjet, electrical discharge machiningflat profiles made from sheet metal, extremely hard materials, prototypesflanges and shaped plates, dies, molds, carbide workpieces
Additive Manufacturingprototypes, one-of-a-kind workpieces, shapes that are impossible to machinemolds, equipment, inserts with internal cooling channels

23.2 Sand-Mold Casting

Casting is the oldest and most flexible method of producing a workpiece: the metal is melted, poured into a mold shaped like the workpiece, and allowed to solidify. The resulting workpiece is called a casting. The most common method for single workpieces and small production runs is sand casting: silica sand mixed with clay and water (green sand) or with resins that harden it.

The Model and the Form

The model is a replica of the workpiece, made of wood, resin, or metal, and slightly larger than the actual workpiece (we’ll see why in section 23.3). It is placed in a frame—the mold—and sand is packed around it. To remove it without damaging the impression, the mold is almost always made of two overlapping halves—the upper and lower halves—which separate along the parting line. The mold is opened, the model is removed, and it is closed again: the cavity remains.

The Souls

The hollow workpieces of the casting (a hole, the interior of a valve body) cannot be formed from the pattern, because the sand around a hole would not be removed. Therefore, asoul: a block of hardened sand, made separately in a soul box, which is placed in the mold before it is closed. The metal flows around it, and when the cast is cool, the core breaks apart and empties out. The core is supported by extensions, the servings, which fit into specific slots in the mold.

Molding and Sprues

The molten metal is poured into the pouring basin, flows down the (vertical) pouring channel, travels through the distribution channels, and enters the mold cavity through the gates. The vents allow air and gases to escape. The risers are reservoirs of molten metal placed above the thickest sections: they solidify last and, as the casting cools, supply the missing metal to the casting. After casting, the casting is removed by breaking the mold (demolding); the gates and risers are cut off; the casting is cleaned by sandblasting or shot blasting; and it is deburred: this is the deburring or finishing of the casting.

molding boxventsprueupper bracketparting linecasting cavitycorelower bracketsprueconnectionsandcompacted
Figure 23.2 · A cross-section of a sand mold, ready for casting. The model has already been removed; what remains is the white cavity, with the core that will form the central hole.
🔥
Approximate casting temperatures. Aluminum alloys are cast at around 700–750 °C, bronzes and brasses at 1000–1150 °C, cast iron at 1300–1400 °C, and steel at 1550–1650 °C. The hotter the metal, the more fluid it is and the better it fills the mold; however, it absorbs more gas, and the mold suffers more as a result. Gray cast iron is the foundry metal par excellence: it melts at a lower temperature than steel, is very fluid, and shrinks very little (Chapter 20).

23.3 Draft, allowance, and draft angles

As the metal cools, it shrinks three times: from a liquid as it cools until it solidifies; during the transition from liquid to solid (between 3 and 7% of the volume, depending on the alloy); and then from a solid, from the solidification temperature down to room temperature. The first two shrinkages are compensated for by the risers, which continue to feed metal into the casting. The third—the linear shrinkage of the solid—is compensated for by making the mold larger.

Cast metalAverage linear retractionUsual field
Reinforcing steel2%1,5-2,5%
Gray cast iron1%0,7-1,2%
Aluminum Alloys1,3%1,0-1,5%
Bronze and Brass1,5%1,2-2,0%

These are approximate, average, and rounded values compiled by us. Actual shrinkage varies depending on the shape of the casting: parts held in place by sand or cores shrink less than those that are free. Gray cast iron shrinks very little because, as it solidifies, it separates graphite, which occupies more volume and partially compensates for the shrinkage.

Model Size
Lm = Lg · (1 + r100)
Lm: measurement on the model in mm · Lg: required length of the cold shot in mm · r: linear shrinkage in %. The model maker works with a model maker's tape measure, which has already been adjusted for shrinkage: it reads “300” where a standard tape measure would read 306.
Example 23.1 · The Same Jet in Three Metals

A casting must be 300 mm long when cold. How long must the mold be if the casting is made of steel, gray cast iron, or an aluminum alloy?

steel (2%): Lm = 300 × 1.02 = 306 mm
gray cast iron (1%): Lm = 300 × 1.01 = 303 mm
aluminum (1.3%): Lm = 300 × 1.013 = 303.9 mm
306 mm, 303 mm, and 303.9 mm: a mold designed for cast iron but cast in steel would result in a casting that is 3 mm shorter

Machining allowance

The surfaces that will later be machined on machine tools are made slightly thicker on the casting; the excess material is called machining allowance. This is necessary because the casting’s surface is hard, contaminated with sand, and full of small defects, and because castings are never precise to the nearest tenth. The ISO 8062 standard defines grades of machining allowance and tolerance; for initial calculations, the values in the table are sufficient.

Sand castingUp to 200 mmFrom 200 to 800 mm
Lightweight Alloys1.5–2.5 mm2.5–4 mm
Gray cast iron2–3 mm3–5 mm
Reinforcing steel3–5 mm5–8 mm

Allowance for each machined surface; approximate values. Apply a thicker layer to the surfaces that face upward during casting, where slag and bubbles accumulate, and significantly reduce the amount in shell molds and die-castings.

The draft angle

A wall that is perfectly perpendicular to the parting line would scrape against the sand when the model is removed and tear it. The walls are therefore inclined by a small draft angle: typically 1° to 2° on the outer walls of sand molds, 2° to 3° on the inner walls, and 0.5° to 2° in metal molds. The draft angle is indicated on the casting drawing; on the finished part, it disappears where the surface is machined.

Expansion Due to Warping
e = h · tan α
and the amount by which the wall shifts at the bottom compared to the top, in mm · h wall height in mm · α draft angle in degrees
finished partallowancedraft angleblank castingmold (casting + shrinkage)The red band represents the allowance; the hatched area represents the pattern, which is larger than the casting after shrinkage.
Figure 23.3 · From the finished part to the model, with exaggerated proportions: an allowance is added to the workpiece, the draft angles are increased, and the entire workpiece is enlarged to account for shrinkage.
Example 23.2 · Dimensions of a Steel Flange Model

A finished cast steel flange has an outside diameter of 200 mm, a thickness of 30 mm, and a hole with a diameter of 80. Machining is performed on all surfaces. A 3 mm allowance is left on each surface; the shrinkage is 2%; and the outer walls have a 1° draft angle. Determine the dimensions of the casting and the pattern.

Blank: diameter 200 + 2 × 3 = 206 mm; thickness 30 + 2 × 3 = 36 mm; hole 80 − 2 × 3 = 74 mm
model: 206 × 1.02 = 210.12 mm; 36 × 1.02 = 36.72 mm
core for the hole (the core box also expands): 74 × 1.02 = 75.48 mm
warpage: e = 36.72 × tan 1° = 36.72 × 0.01746 = 0.64 mm per side
Diameter of the model at its widest point: 210.12 + 2 × 0.64 = 211.40 mm
Casting Ø206 × 36 with a hole Ø74; model Ø210.1 (211.4 on the wide side) × 36.7, core Ø75.5

Pay attention to the hole: the allowance is removed from the diameter of the hole, because the blank hole must be smaller than the finished hole.

23.4 Other Foundry Processes and Casting Defects

The sand mold breaks with every casting. For mass production, permanent molds or processes that produce more precise castings are used:

  • shell molding: The mold is made of steel or cast iron and can withstand thousands of castings; the metal flows in by gravity (or under low pressure, as in car rims). The metal cools quickly against the cold wall, resulting in a fine grain: castings that are stronger and more precise than those made with sand. This method is particularly suitable for aluminum and copper alloys;
  • Die casting: Liquid metal is injected at high pressure (hundreds of bar) into a cooled steel mold in a matter of hundredths of a second. Thin walls as thin as 1–2 mm, excellent tolerances, cycles of one minute or less: housings, casings, and bodies of power tools made of aluminum, zamak (zinc alloy), and magnesium. Castings may have internal porosity caused by trapped gas; for this reason, they are usually not welded or heat-treated;
  • lost-wax casting: A wax model is made (injected into a mold), covered with layers of ceramic material, the wax is melted away, and the metal is poured into the hot shell. No parting lines, extremely fine details, almost no further machining operations required: turbine blades, weapon workpieces, prosthetics, jewelry, small workpieces made of stainless steel or superalloys;
  • Centrifugal casting: The mold rotates rapidly around its axis, and the metal is forced against the outer wall. This produces solid, coreless tubes and rings, with the (lighter) impurities collected inside, where they are then turned away: cast iron tubes, cylinder liners, and bronze bushings.
ProcessCommon MetalsTolerance (100-mm workpiece)Ra (µm)Series
Sandeveryone± 1–2 mm12,5-25Single workpieces, small and medium-sized production runs
Shellaluminum, copper± 0.3–0.8 mm3,2-6,3medium-sized series
Die Castingaluminum, zinc, magnesium± 0.1–0.3 mm0,8-3,2large-scale production
Lost-wax castingsteel, stainless steel, superalloys± 0.2–0.5 mm1,6-3,2small and medium-sized production runs
Centrifugecast iron, steel, bronze± 1–2 mm (to be turned later)6,3-12,5tubes, rings, bushings

Approximate values for comparing processes, compiled by us; actual tolerances depend on dimensions and shape (ISO 8062).

Defects in Castings

Anyone who processes castings on machines encounters them all, often right beneath the first pass. Knowing what they are helps you determine whether a workpiece should be rejected and lets the foundry know what needs to be corrected.

DefectWhat It Looks LikeMain cause
Blowinground, smooth blisters, often near the top surfacegas from the metal or wet sand that cannot escape
Shrinkage cavities (pits)hollows with rough, jagged walls in the thickest areasThe ingot is too small or improperly positioned: metal is missing as it solidifies
Porositymany small holes scattered throughout, which become visible after machiningdissolved gas, diffuse shrinkage; typical of die casting
Inclusionsgrains of sand or slag inside the metal; they damage the insertsloose sand, slag not retained by the basin
Cold jointa line where two streams of metal touched without fusing togetherThe metal is too cold, or the flow is too slow
Incomplete castthin, unfilled sectionsmetal that doesn't flow well, walls that are too thin, insufficient vents
Hot cracksirregular cracks, often at the sharp edges between thick and thin sectionsContraction prevented by the mold or the core while the metal is still soft
OffsetThe two halves of the cast do not coincide on the plane of division.Improperly secured clamps or worn-out centering pins
✅
Designing for the foundry. Wall thicknesses should be as uniform as possible, with gradual transitions between thick and thin sections, generous fillets instead of sharp edges, and no isolated sections far from the risers. A well-designed casting has few defects from the start, and is easier to work with.

23.5 Plastic Deformation: Hot and Cold

When a metal is loaded beyond its yield point, it deforms permanently (Chapter 19): layers of atoms slide over one another, the workpiece changes shape but does not break, and its volume remains the same. This is the principle behind forging, rolling, extrusion, wire drawing, and all sheet metal machining operations.

Work Hardening

As it is deformed at room temperature, the metal becomes harder and stronger but less ductile: this is work hardening, the same upward slope seen in the tensile test after yield. A copper wire bent back and forth becomes stiff and then breaks; cold-rolled sheet metal is stronger than hot-rolled sheet metal. Work hardening is used to strengthen materials that cannot be heat-treated (copper, 5000 series aluminum, austenitic stainless steels; see Chapters 20 and 21), but it has a limit: beyond a certain degree of deformation, the metal cracks. To continue, annealing is required, which restores the metal’s ductility (Chapter 22).

The recrystallization temperature

If the metal is hot enough, the deformed grains reform as the metal is deformed: this is recrystallization. Work hardening disappears as it occurs, the metal remains soft, and it can be deformed significantly with small forces. The temperature above which this occurs is approximately 40% of the melting point, measured in kelvins:

Recrystallization temperature (estimate)
Tr ≈ 0,4 · Tf T (K) = T (°C) + 273,15
Tr is the recrystallization temperature in K; Tf is the melting temperature in K. The coefficient ranges from 0.3 to 0.5: it decreases in very pure metals and when the prior deformation is severe. This is an estimate to understand the order of magnitude.

Hence the key definition: a machining operation is considered hot if it is performed above the recrystallization temperature, and cold if it is performed below it. It does not depend on how “hot” the workpiece feels to the touch.

Example 23.3 · Hot or cold?

Estimate the recrystallization temperature of lead (melts at 327.5 °C), aluminum (660.3 °C), iron (1538 °C), and tungsten (3422 °C).

lead: 0.4 · (327.5 + 273.15) = 0.4 · 600.65 = 240.3 K = −32.9 °C
aluminum: 0.4 · (660.3 + 273.15) = 0.4 · 933.45 = 373.4 K = 100.2 °C
iron: 0.4 · (1538 + 273.15) = 0.4 · 1811.15 = 724.5 K = 451.3 °C
tungsten: 0.4 · (3422 + 273.15) = 0.4 · 3695.15 = 1478.1 K = 1204.9 °C
Lead that has been crushed at 20 °C is hot-worked (it does not work-harden); tungsten drawn into wire at 1000 °C is cold-worked
Immediately afterCold
Forces and Deformationslow forces, enormous deformations in a single stepHigh forces, limited deformation before annealing is required
Areacovered with oxide (scale or calamine)shiny and clean
Accuracylow: the workpiece shrinks as it coolshigh: tolerances of a few cents (drawn bars h9, Chapter 20)
Workpiece Propertiesre-milled and refined grain, no work hardeningwork-hardened: stronger, less ductile, with internal stresses
Typical temperaturessteel 900–1,250 °C · brass 650–800 °C · aluminum 350–500 °C · titanium 850–1,000 °Croom temperature

Approximate hot machining operations temperatures, rounded.

Percentage reduction (degree of deformation)
ε = h0 − h1h0 · 100 εA = A0 − A1A0 · 100
h0, h1: thickness before and after, in mm · A0, A1: cross-sectional area before and after, in mm² · ε: in %. The greater the cold reduction, the more the metal work-hardens.

23.6 Forging and Hot Forming

Forging shapes hot metal by striking it with a hammer or applying pressure with a press. In open die forging, the workpiece is placed between two plates (or simple tools), and the blacksmith or operator rotates and moves it: it is stretched (stretching), shortened while being widened (re-forging), pierced, or bent. This is the method used to make large shafts, rings, and one-of-a-kind workpieces weighing up to many metric tons.

Why is a forged workpiece more durable?

Rolled steel is not uniform in all directions: impurities and inclusions have been elongated during rolling and form fibers, much like the grain of wood. The material is stronger along the fibers than across them. If the workpiece is machined from solid stock using a milling machine or lathe, the fibers are cut where the cross-section changes—precisely where the stresses are highest. If, on the other hand, the workpiece is forged, the fibers bend and conform to the shape: this is why connecting rods, shafts, hooks, and high-quality wrenches are forged or stamped.

fibers cut at an edgemachined from a solid barforged: the fibers follow the shape
Figure 23.4 · The same shape, but with a head wider than the stem. On the left, the fibers of the bar are cut at the fillet between the head and the stem; on the right, in the traced workpiece, they run inside the head without interruption.

Molding and Flash

In hot forging, the blank—a section of bar heated to red-hot—is pressed between two steel dies that bear the shape of the finished workpiece. A little more metal than necessary is always used: the excess flows out between the two dies, forming a thin sheet known as the flash. Because the flash is thin, it cools quickly, creating resistance and forcing the rest of the metal to fill all the corners of the impression; any remaining excess metal ends up in the flash channel. After stamping, the flash is removed using a flash trimmer, a small press equipped with a shearing die. Often, the workpiece passes through several successive dies (roughing, semi-finishing, finishing) before reaching its final shape.

workpieceFmolduppermoldlowerflashsprueof the flashThe excess metal flows out between the two mold halves, cools into a thin strip, and holds back the rest, which fills the cavity.
Figure 23.5 · Dies closed at the end of the travel. The red metal is the workpiece with the burr, which is later removed by the deburring machine.

Castings also have draft angles (ranging from 3° to 7° on the outer walls, and more on the inner walls) and machining allowances for subsequent machining operations, usually ranging from 1 to 3 mm. To calculate the blank weight, start with the workpiece’s volume and add the burr and the metal lost as oxide (shrinkage).

Example 23.4 · The bar segment for a stamped workpiece

A stamped steel lever weighs 1.2 kg after deburring. The burr accounts for 12% of the workpiece’s mass, and heat shrinkage accounts for 3%. What length of Ø40 bar must be cut? (Density of steel: 7.85 kg/dm³)

Mass of the piece: 1.2 × 1.12 × 1.03 = 1.384 kg
volume: 1.384 / 7.85 = 0.1763 dm³ = 176,350 mm³
cross-sectional area of the bar: π · 40² / 4 = 1256.6 mm²
length: 176,350 / 1,256.6 = 140.3 mm
Pieces approximately 140 mm long cut from a Ø40 bar

23.7 Lamination

In rolling, the metal is passed between two cylinders rotating in opposite directions: friction pulls it in, and the gap between the cylinders—which is narrower than the workpiece—flattens it. It is the process that produces the most metal in the world: slabs and billets from the steel mill (Chapter 20) are transformed into sheet metal, strip, bars, beams, rails, and wire rod. Hot rolling achieves the largest reductions in thickness; cold rolling, applied to strips that have already been pickled, produces thin, precise, and polished sheets. Shaped rolls (dies) are used to produce round bars, square bars, double-T beams, and structural sections.

Rαh0h1v0v1upper cylinderlower cylinderincoming sheetrolled sheet metal
Figure 23.6 · The sheet enters with a thickness of h0 at a speed of v0 and exits with a thickness of h1, moving faster. α is the contact angle between the sheet and the cylinder of radius R.

The volume remains constant: if the thickness decreases, the length (and, to a lesser extent, the width) increase. In wide sheets, the increase in width is small and can be neglected. The flow rate of metal is also the same at the inlet and outlet, so the sheet exits faster than it enters.

Preservation of the Laminated Volume
h0 · b0 · L0 = h1 · b1 · L1
with constant b: L1 = L0 · h0h1 v1 = v0 · h0h1
h = thickness · b = width · L = length, all in mm · v = material speed in m/s or m/min · subscript 0 for input, 1 for output
Example 23.5 · How much does a rolled plate elongate?

A 40 × 120 mm plate, 1,500 mm long, is rolled to a thickness of 25 mm. Expansion is neglected. Find the final length, the percentage reduction, and the exit speed if the plate enters at 1 m/s.

L1 = 1500 × 40 / 25 = 2400 mm
reduction: (40 − 25) / 40 × 100 = 37.5%
v1 = 1 · 40 / 25 = 1,6 m/s
Volume check: 40 × 120 × 1,500 = 7,200,000 mm³ and 25 × 120 × 2,400 = 7,200,000 mm³ ✓
2.4 m in length, 37.5% reduction, exit velocity of 1.6 m/s

How much can it be reduced in one pass?

The rollers “grip” the sheet metal only if there is sufficient friction to pull it in: the contact angle α must not exceed the coefficient of friction, that is, tan α ≤ μ. This leads to a simple rule for the maximum thickness reduction in a single pass:

Grip Condition
since α = 1 − Δh2 · R tan α ≤ μ Δhmax ≈ μ² · R
Δh = h0 − h1 thickness reduction in mm · R radius of the cylinders in mm · μ coefficient of friction between the cylinder and the metal (approximately 0.05–0.1 when cold with lubricant, 0.2–0.4 when hot) · α contact angle
Example 23.6 · Do the cylinders hold the plate?

In Example 23.5, the cylinders have a radius of 300 mm and are hot-rolled with μ = 0.3. Is a reduction of 15 mm possible in a single pass?

Δhmax ≈ 0.3² · 300 = 0.09 · 300 = 27 mm
Calculation using the angle: cos α = 1 − 15/600 = 0.975 → α = 12.84°; friction angle: arctan 0.3 = 16.70°
Yes: 15 mm is less than the possible 27 mm, and α = 12.8° is less than 16.7°

In cold rolling, with μ = 0.08, the same rolling mill would process a maximum of 0.08² × 300 = 1.9 mm; for this reason, cold rolling is carried out in small reductions over many passes.

23.8 Extrusion and Drawing

Extrusion

In extrusion, a hot metal cylinder—the billet—is placed in a chamber, and a piston pushes it through the shaped hole of a die, much like toothpaste coming out of a tube. The result is a long profile with the same cross-section as the hole. This is the process used to produce aluminum profiles (windows and doors, structural machine profiles, heat sinks), copper and brass tubes, and brass bars for automatic turning. Hollow profiles can also be produced using special dies.

barFdiepistoncontainerextruded profileDirect (hot) extrusionFd0d1dieWire drawing (cold)
Figure 23.7 · On the left, the piston pushes the billet through the die. On the right, the wire is drawn through the conical hole in the draw die and tapers.
Extrusion ratio (reduction ratio)
R = A0A1 L1 = L0 · R v1 = vp · R
A0 billet cross-sectional area · A1 profile cross-sectional area, in mm² · L0 length of the extruded billet · L1 length of the profile, in mm · vp piston speed · v1 profile speed. For aluminum, R typically ranges from 10 to 100. In practice, a small portion of the billet (the end piece) remains in the die and is discarded.
Example 23.7 · From a billet to a bar

An aluminum alloy billet with a diameter of 120 and a length of 400 mm is extruded into a round bar with a diameter of 30. The piston moves forward at 10 mm/s. Find the extrusion ratio, the length of the bar (ignoring the end cap), and the exit velocity.

Circle on circle: R = (120 / 30)² = 4² = 16
L1 = 400 × 16 = 6,400 mm
v1 = 10 × 16 = 160 mm/s = 9.6 m/min
R = 16, a 6.4-meter bar extending at 9.6 m/min

Extrusion

In wire drawing, the material is not pushed but pulled through a carbide or diamond die with a conical hole. The process is performed cold, so the reduction per pass is limited: if too much force is applied, the wire breaks as it exits. Typically, the cross-sectional area is reduced by 15 to 35 percent per pass, and multiple passes are performed in succession, with intermediate annealing when the material becomes too work-hardened. Wire drawing is used to produce wires, polished calibrated bars (Chapter 20), and precision tubes.

Number of drawing passes
n = ln (A0 / An) ln (1 / (1 − q)) rounding: A0An = d0²dn²
n: number of passes (rounded up) · A0, An: initial and final cross-sectional areas · q: permissible reduction in cross-sectional area per pass, as a decimal number (0.25 = 25%) · ln: natural logarithm (Chapter 1)
Example 23.8 · How many passes from Ø6 to Ø4

A Ø6 steel wire must be reduced to Ø4, with a maximum cross-sectional reduction of 25% per pass.

ratio of the cross-sectional areas: 6² / 4² = 36 / 16 = 2.25 (total reduction of 55.6%)
n = ln 2.25 / ln (1 / 0.75) = 0.8109 / 0.2877 = 2.82 → 3 passes
with 3 equal passes; each pass divides the section by ∛2.25 = 1.3104, that is, it reduces it by 23.7%
diameters: 6 → 6 / √1.3104 = 5.24 → 4.58 → 4.00 mm
3 passes: Ø6 → Ø5.24 → Ø4.58 → Ø4, each with a 23.7% reduction

23.9 Sheet Metal: Blanking and Punching

Blanking involves cutting a workpiece out of a sheet of metal using a descending punch and a die positioned below it, both mounted in a die set on the press. We refer to blanking when the finished workpiece is the workpiece that falls into the die (a disc, a shape), and to punching when the finished workpiece is the sheet metal that remains and the workpiece that falls out is the scrap (a hole, a slot). We already covered the calculation of force in Chapter 10, in the context of shear strength.

How to detach the workpiece

The punch first presses down on the sheet metal and bends it slightly (creating a rounded edge), then cuts it along a section, leaving a shiny band (the smooth area, about one-third of the thickness in mild steel); finally, the material tears along a line running from the edge of the punch to that of the die (the fracture zone, which is dull and slanted). A small burr remains on the die side. If the clearance between the punch and the die is correct, the two cracks starting from the two edges meet, and the cut is clean.

stampFsheet metal presssheet metaldieclearance g per sidethe disc falls herescut edge (enlarged)roundingsmooth areafracture zoneburrThe red dashed line indicates where the material tears
Figure 23.8 · On the left, a cross-section of the die: the punch is smaller than the die hole by a clearance of g on each side. On the right, the edge of a stamped workpiece, showing its four zones.

Shear force

Shearing Force
F = p · s · τR τR ≈ 0.8 · Rm disk or hole: p = π · d
F force in N · p cut perimeter in mm (the sum of all contours cut in the same pass) · s sheet thickness in mm · τR shear strength in N/mm² · Rm tensile strength in N/mm² (Chapter 19) · d diameter in mm

The rated force of the press (in kN, or in “metric tons” of force: 1 t ≈ 9.81 kN) is selected with a margin, usually 20–30% higher, partly because the force required to remove the sheet metal from the punch (extraction force, 5 to 10% of F), provided by the spring-loaded sheet metal holder, is added to the shearing force. Work is also a factor: a mechanical press derives it from the flywheel, and if the required work is too great, the flywheel slows down and the press stalls.

Shearing Operations and Press Force
W = λ · F · s Fpress ≥ 1,2 · F
W work in N·mm (divided by 1000 gives joules) · λ fraction of the thickness over which the punch operates at full force before fracture: approximately 0.5 for mild steel, less for hard and brittle materials, and more for soft materials · F: shearing force in N
Example 23.9 · Slicing a disk

Discs with a diameter of 50 are cut from 2-mm-thick S235 sheet metal (Rm ≈ 400 N/mm²). Determine the force, the work, and the minimum press force.

τR ≈ 0.8 × 400 = 320 N/mm²
F = π · 50 · 2 · 320 = 314.16 · 640 = 100,531 N ≈ 100.5 kN
W = 0.5 × 100,531 × 2 = 100,531 N·mm ≈ 100.5 J
Pressure: 1.2 × 100.5 = 120.6 kN, or 120,600 / 9,810 = 12.3 metric tons
F ≈ 100 kN; a press with a capacity of at least 12.5 metric tons is required (in practice, a 16- or 20-metric-ton press, based on standard commercial sizes)

The Clearance Between Punch and Die

The clearance begins per side, as a percentage of the thickness. If it’s too small, the two cracks won’t meet, the punch makes two cuts, and it wears out quickly; if it’s too large, the edge rounds off significantly and the burr grows. Where to set the clearance depends on which workpiece is the good one:

  • blanking (the good workpiece is ejected): the workpiece is cut to the size of the die, so the die is made to the size of the workpiece, and the punch is 2g smaller;
  • Punching (the good workpiece is the hole): The hole is made to fit the punch, so the punch is made to fit the hole, and the die is 2g larger.
Play on the wing
g = c · s shearing: Dpunz = D − 2g punching: dmatr = d + 2g
g: clearance per side in mm · c: material coefficient (table), as a decimal number · s: thickness in mm · D: diameter of the workpiece = diameter of the die · d: hole diameter = diameter of the punch
Sheet Metal MaterialClearance on the wing (% of clearances)
Soft aluminum3-5%
Copper and Brass4-6%
Mild steel (DC01, S235)5-7%
Medium-hard steel (S355, C45)6-8%
Stainless steel7-10%

These are approximate values for sheet metal up to 3–4 mm thick, compiled by us. Mold makers use their own tables, and for high-quality edges (fine blanking), they work with much smaller clearances.

Example 23.10 · Dimensions of punches and dies for a washer

A 2-mm-thick mild steel washer has a hole with a diameter of 10 and an outer diameter of 22. A 6% clearance is allowed on each side.

g = 0.06 × 2 = 0.12 mm per side
hole (punching): punch Ø10.00; die 10 + 2 × 0.12 = Ø10.24
external (blanking): die Ø22.00; punch 22 − 2 × 0.12 = Ø21.76
Hole: punch Ø10 and die Ø10.24 · exterior: die Ø22 and punch Ø21.76
Example 23.11 · A shaped plate with four holes

A die cuts a rectangular plate measuring 80 × 40 mm with four Ø8 holes from a 3-mm-thick sheet of S355 steel (Rm ≈ 500 N/mm²) in a single stroke.

outer perimeter: 2 · (80 + 40) = 240 mm
holes: 4 · π · 8 = 100.53 mm → total perimeter p = 340.53 mm
τR ≈ 0.8 × 500 = 400 N/mm²
F = 340.53 × 3 × 400 = 408,637 N ≈ 409 kN (41.7 t)
Pressure: 1.2 × 408,637 = 490,364 N → 490,364 / 9,810 = 50.0 t
Work: W = 0.5 × 408,637 × 3 = 612,956 N·mm ≈ 613 J
Approximately 409 kN of force: a 50-metric-ton press is needed, capable of delivering at least 613 J per stroke

To use a smaller press, you can stagger the length of the punches (first the holes, then the outline, so the two forces do not add up) or give the cutting edges aninclination (shearing), so that the cut is made little by little, just like with scissors.

23.10 Sheet Metal Bending

During bending, the sheet metal deforms along a straight line. In the bend area, the outer fibers stretch (they are under tension), while the inner fibers shorten (they are under compression); between the two is a fiber that does not change in length: the neutral fiber. It is this fiber that determines how long the flat sheet must be before bending—that is, the developed length.

rcompressed fibers (inside)stretched fibers (outer layer)neutral fibersbadistance of the neutral fiberfrom the inside of the fold: K · s
Figure 23.9 · A 90° bend with an inner radius r and thickness s. The neutral fiber (red hatching) neither stretches nor shortens: its arc is included in the net.

In a bent sheet, the neutral axis does not lie at the midpoint of the thickness but slightly toward the inside, because the compressed material thickens and the stretched material thins. Its position is given by the K-factor: the neutral axis lies at a distance of K · s from the inner face.

R/S ratioK-factor
up to 10,33
1 to 30,40
more than 30,50

Approximate values for mild steel bent in air. Sheet metal CAD programs and press brake tables provide their own values, which are often calibrated using test bends: if the development must be accurate to a tenth, bend a sample and adjust K.

Development of a Folded Sheet Metal Part
L = Σ straight segments + Σ π · α180 · (r + K · s)
90° bend: arc = π2 · (r + K · s) straight segment = outer side − (r + s) for each nearby fold
L: development in mm · α: bend angle in degrees · r: inner radius of the bend in mm · s: thickness in mm · K: neutral fiber factor. Dimensions are usually specified on the outside: from each side, subtract the portion that lies on the bend, i.e., r + s.
Example 23.12 · The Construction of an L-Bracket

An L-shaped bracket has outer sides measuring 50 and 30 mm, a thickness of 3 mm, and an inner radius of 4.5 mm. Find the length of the flat workpiece.

r / s = 4,5 / 3 = 1,5 → K = 0,40
Straight segments: 50 − (4.5 + 3) = 42.5 mm and 30 − 7.5 = 22.5 mm
arc: π/2 · (4.5 + 0.40 · 3) = 1.5708 · 5.7 = 8.95 mm
L = 42.5 + 22.5 + 8.95 = 73.95 mm
Cut a strip 73.95 mm long (about 74 mm), not 80 mm, which is the sum of the outer sides
6040s = 2r = 3 (internal)3550355.975.97development 131.94The arcs of the neutral fiber are shown in red; the rest are straight segments
Figure 23.10 · The U-shaped profile from Example 23.13 (external dimensions in mm) and its flat strip: three straight sections and two neutral-fiber arcs.
Example 23.13 · The Development of a U-Shaped Profile

A U-shaped profile has an outer base of 60 mm, outer flanges 40 mm high, a thickness of 2 mm, and an inner radius of 3 mm.

r / s = 3 / 2 = 1,5 → K = 0,40
wings: 40 − (3 + 2) = 35 mm each; base: 60 − 2 · (3 + 2) = 50 mm (two adjacent folds)
one arc: π/2 · (3 + 0.40 · 2) = 1.5708 · 3.8 = 5.97 mm; two arcs: 11.94 mm
L = 35 + 35 + 50 + 11.94 = 131.94 mm
Unfolded length 131.94 mm: on the flat workpiece, the fold lines are 35 + 2.98 = 37.98 mm from each end

Minimum radius and rolling direction

If the inner radius is too small, the outer fibers stretch too much and the sheet metal cracks at the bend. The minimum radius depends on the material and its condition, and is expressed as a multiple of the thickness. Whenever possible, the bend should be made across the direction of rolling: if bent along the grain, the sheet will crack sooner.

MaterialMinimum inside radius (90° bend)
DC01 mild steel, S2350,5-1 · s
S355 Steel1-1,5 · s
Austenitic stainless steel (1.4301)0,5-1 · s
Annealed brass and copper0,5-1 · s
5754 H22 Aluminum1-1,5 · s
6082 T6 Aluminum3–4 · s (tends to crack: best when annealed)

Approximate values, compiled by us, for thicknesses up to approximately 6 mm and transverse bending during rolling.

Elastic Recovery

When the punch rises, the elastic portion of the deformation recoils and the bend opens slightly: this is elastic recovery. It is greater the higher the material’s strength is relative to its stiffness (high Re, low E) and the larger the radius is relative to the thickness. Generally speaking, it ranges from 1–2° for mild steel to 2–4° for stainless steel and 3–6° for hard aluminum. This is compensated for by bending slightly beyond the desired angle or by compressing the bend at the bottom of the die (coining); modern bending machines measure the angle with a sensor and correct it automatically.

Bending Force in a V-Die

In a press brake, the sheet metal rests on the two edges of a V-shaped die, and the punch pushes it down in the center. In air bending, the sheet metal does not touch the bottom of the V: the angle depends on how far the punch descends, and the resulting inner radius is approximately one-sixth of the V-opening. The opening is usually chosen to be 8 times the thickness (from 6 to 12): the wider the opening, the less force is required, but the larger the radius becomes.

FpunchV-dieVsheet metalafter the returnelasticflat sheet metal
Figure 23.11 · Air bending: The sheet metal touches only the tip of the punch and the two edges of the die. The red dashed lines show the bend, which opens slightly as the punch rises.
Bending force in air (practical formula)
F ≈ 1,33 · L · s² · RmV
F force in N · L bend length in mm · s thickness in mm · Rm tensile strength in N/mm² · V die opening in mm. This is a workshop formula, valid for 90° bends in free air with V ranging from 6 to 12 times s; the tables provided by bending machine manufacturers give very similar values. In coining, the force is 3 to 5 times greater.
Example 23.14 · Is a bending machine enough?

A 3-mm-thick, 1-meter-long sheet of S235 steel (Rm ≈ 420 N/mm²) must be bent to a 90° angle. The press brake has a capacity of 40 metric tons.

opening: V = 8 × 3 = 24 mm
F = 1.33 × 1000 × 3² × 420 / 24 = 5,027,400 / 24 = 209,475 N ≈ 209 kN
in metric tons: 209,475 / 9,810 = 21.4 metric tons
resulting inner radius: approximately 24 / 6 = 4 mm
It takes about 21 metric tons per meter: the 40-metric-ton press brake is sufficient, and it could bend up to nearly 1.9 meters of that sheet metal

23.11 Deep Drawing and Calendering

Through deep drawing, a flat disc is transformed into a hollow workpiece: a glass, a pot, a can, a compressor tank, or a fender. The disc rests on the die; a sheet metal presser holds it in place, and the punch pushes it into the hole in the die. The edge of the disc moves toward the center: its circumference shrinks, and it tends to wrinkle, which the sheet metal presser prevents. If the sheet metal presser clamps too tightly, however, the bottom of the glass tears near the radius of the punch.

punchsheet metal pressdieDdhdeep-drawn glass
Figure 23.12 · On the left, the disc with diameter D, ready beneath the punch; on the right, the cup with diameter d and height h that is formed from it.

The Starting Disc

In deep drawing, the thickness remains almost the same (it decreases slightly at the bottom radius and increases slightly at the rim), so it can be said that the surface area is preserved: the surface area of the disc is equal to that of the glass. For a cylindrical glass, neglecting the fillets:

Disc diameter for a cylindrical glass
π · D²4 = π · d²4 + π · d · h → D = √(d² + 4 · d · h)
D: disc diameter in mm · d: cup diameter in mm (for thick sheets, use the average diameter, which is half the thickness) · h: cup height in mm, including the rim that will later be trimmed. On the left is the surface area of the disc; on the right is the surface area of the bottom plus that of the sidewall.

The ratio β = D / d is called the deep-drawing ratio. In a single operation, a certain limit value cannot be exceeded, the limit deep-drawing ratio, which for deep-drawing steels and stainless steel is approximately 1.8–2.0 (up to 2.1 for the highest-quality sheets) and for aluminum is approximately 1.7–1.9. If the cup is deeper, multiple operations (re-drawing) are performed, each with a smaller ratio, ranging from 1.2 to 1.3, and intermediate annealing is performed if necessary.

Example 23.15 · The coaster for a glass

A cylindrical glass with a diameter of 60 mm and a height of 40 mm, made of deep-drawing steel (β limit = 2.0), must be deep-drawn. Allow 3 mm in height for trimming the rim.

height for deep drawing: 40 + 3 = 43 mm
D = √(60² + 4 × 60 × 43) = √(3,600 + 10,320) = √13,920 = 117.98 mm
β = 117,98 / 60 = 1,97 ≤ 2,0 ✓
Disc Ø118: The cup is formed in a single operation, but just barely (without trimming, D would be 114.9 mm and β would be 1.91)

Calendering

Calendering bends a sheet or profile by passing it between three (or four) rollers: two fixed rollers at the bottom and one adjustable roller at the top, which pushes and bends the material. Pass after pass, as the roller is lowered, the sheet metal takes on an increasingly smaller radius until it forms a cylinder (tube) or a cone. This process is used to make large welded tubes, tanks, silos, flange rings, and machine frames. The ends of the sheet metal remain straight for a section (the rollers do not bend them): they are pre-bent first using a press or the four-roller calender itself.

23.12 Thread Rolling and Sintering

Thread rolling

Screws can be threaded by cutting the material (on a lathe, with a die, or with a tap; see Chapter 28) or by rolling it: two or three hardened rollers, which carry the negative profile of the thread, press against the round bar and rotate, cold-deforming it. The material displaced from the bottom of the threads rises to form the crest. Almost all commercial screws are rolled.

cut thread: broken fibersrolled fillet: continuous fibersand compressed thread base
Figure 23.13 · Cross-section of two threads. In the cut thread, the fibers of the bar run perpendicular to the flank; in the rolled thread, they bend and follow the profile.

The rolled thread is superior for three reasons: the fibers are not cut but follow the profile (as in a forged workpiece), the base of the thread is work-hardened and compressed and therefore resists fatigue much better (Chapter 22), and the surface is smooth. Plus, it’s extremely fast and produces no chips. Since the material moves without being lost, the round bar to be rolled is selected to be approximately equal to the average diameter of the threads, not the nominal diameter.

Diameter of the round bar to be rolled (metric threads)
dtondo ≈ d2 = d − 0.6495 · P
d nominal screw diameter in mm · P pitch in mm · d2 average thread diameter (Chapter 17). This is a starting value: the roller manufacturer refines it through testing.
Example 23.16 · The round piece for rolling an M10

Rolled M10 × 1.5 screws: What is the diameter of the round bar that is turned or drawn?

d2 = 10 − 0.6495 × 1.5 = 10 − 0.974 = 9.026 mm
Round bar, approximately Ø9.03: after rolling, the crest reaches Ø10

Powder Metallurgy

In sintering, the workpiece is formed from a metal powder (iron, alloy steels, bronze, stainless steel) mixed with a lubricant. The process consists of three stages:

  • pressing: the powder is poured into a mold and compressed with punches at pressures of 400–800 N/mm²; the “green” workpiece already has its shape but is fragile, like plaster;
  • sintering: the green workpiece is heated in a furnace, in a protective atmosphere, to approximately 70–80% of the melting temperature (1120–1150 °C for iron); the particles bond together without melting;
  • Calibration and finishing: A second pressing restores the precise dimensions; if necessary, the piece is oiled, heat-treated, or machined.

Sintered workpieces come out fully finished, with tolerances of just a few hundredths and almost no material waste: oil pump gears, pawls, cams, lock parts, and power tool components. They remain somewhat porous: this limits their strength, but becomes an advantage in self-lubricating bushings, whose pores fill with oil. The parts must be able to be removed from the mold vertically (no undercuts), and production runs must be large, because the mold is expensive.

Porosity of a Sintered Material
P = (1 − ρρfull) · 100
P porosity as a percentage of volume · ρ density of the sintered material · ρfull density of the solid metal, in the same unit (g/cm³)
Example 23.17 · A self-lubricating bushing

A sintered bronze bushing has an outer diameter of 20, a hole diameter of 12, and a length of 15 mm. Its density is 6.4 g/cm³, while that of compact bronze is 8.8 g/cm³. Find the porosity and the mass.

P = (1 − 6,4 / 8,8) · 100 = (1 − 0,7273) · 100 = 27,3%
volume: π/4 · (20² − 12²) · 15 = 0.7854 · 256 · 15 = 3,015.9 mm³ = 3.016 cm³
mass: 3.016 × 6.4 = 19.3 g
27% porosity, which fills with oil; the bushing weighs 19.3 g

23.13 Non-Conventional Machining Operations

Unconventional machining operations are those that remove material without a tool that chips away material with a cutting edge: they use the heat of a light beam, an electric arc, or a flame; the force of a water jet; or electrical discharges. They are not dependent on the hardness of the material and do not exert pressure on the workpiece; for this reason, they can cut thin sheet metal without deforming it and machine hardened steels and cemented carbide.

Laser Cutting

A laser beam, focused by a lens into a spot measuring a few tenths of a millimeter, melts and vaporizes the metal; a gas emerging from the coaxial nozzle blows away the molten material. With oxygen, the steel burns, and cutting is faster on thicker materials, but the edge remains oxidized; with nitrogen, the edge remains clean and shiny, ready for painting or welding (stainless steel, aluminum). Today, almost all machines use fiber lasers, ranging from 2 to over 20 kW. The kerf is narrow (0.1 to 0.4 mm), the heat-affected zone is small, and tolerances are in the range of ± 0.05–0.1 mm.

Thickness of non-alloy steel1 mm3 mm6 mm10 mm20 mm
Cutting speed (m/min)25-355-82,5-31,2-1,60,5-0,7

Order-of-magnitude figures for a fiber laser of approximately 4 kW, compiled by us. Actual speeds depend on the source, the gas, and the desired edge quality; these are provided in the machine manufacturer’s tables.

Cutting time for a sheet of metal
t = Lv + n · tsf
t time in minutes (× 60 for seconds) · The total length of the cut contours in mm · v cutting speed in mm/min · n number of cuts (one for each contour) · tsf time per cut in min. Rapid traverse movements between contours are then added.
Example 23.18 · How long does the laser take?

A 600 × 400 mm plate with 12 holes (Ø20) is cut from 3 mm-thick steel sheet at a speed of 5 m/min. Each punch takes half a second.

outer perimeter: 2 · (600 + 400) = 2000 mm
holes: 12 · π · 20 = 753.98 mm → L = 2753.98 mm
Calculation: 2753.98 / 5000 = 0.5508 min = 33.0 s
breakthroughs: 13 · 0.5 = 6.5 s
About 39.5 seconds plus the quick cuts: less than a minute for a workpiece that would take an hour to do by hand, using a drill and a hacksaw

Plasma and Oxy-Fuel Cutting

Plasma cutting uses an electric arc between an electrode and the workpiece, constricted by a narrow nozzle: the gas passing through it becomes plasma at over 20,000 °C and melts the metal. It cuts all metals that conduct electricity, is fast on medium-thickness materials (up to 30–50 mm), and the machine costs less than a laser; however, the kerf is wide (1.5–4 mm), the edge is slightly beveled, and the cut is less precise (± 0.3–0.5 mm). Oxy-fuel cutting heats the steel with a flame to its ignition temperature and then burns it with a jet of pure oxygen: it works only on carbon and low-alloy steels (not on stainless steel, aluminum, copper, or cast iron), but it can cut extremely thick materials—even over 300 mm—using simple equipment. The heat-affected zone is large, and the workpiece often requires finishing.

The Water Jet

A pump pressurizes the water to 4,000–6,000 bar and shoots it through a sapphire nozzle just a few tenths of a millimeter in diameter; for hard materials, abrasive sand (garnet) is added. The water jet cuts through any material: metals, titanium, stone, glass, ceramics, composites, rubber, and food. It does not heat the workpiece, so it does not deform it or alter its structure: it is the right choice for heat-sensitive materials and for hardened workpieces. It is slower than a laser on thin metals.

Electrical Discharge Machining

Electrical discharge machining (EDM) removes material through thousands of tiny electrical discharges per second between an electrode and the workpiece, which are immersed in an insulating liquid (the dielectric). Each spark melts and vaporizes a tiny crater; the dielectric cools and carries away the particles. The electrode and workpiece never touch: a small space, known as the gap (or spark gap), remains between them. It works only on materials that conduct electricity, regardless of how hard they are: steels hardened to 60 HRC, cemented carbide, and titanium.

  • Wire cutting: The electrode is a brass wire (Ø 0.1–0.3 mm) that continuously runs between two guides and cuts through the workpiece from one side to the other, like a scroll saw, in deionized water. The guides can be moved relative to one another to cut inclined walls (die draft angles) and different profiles on the top and bottom. One roughing pass and two or more finishing passes are used: tolerances of ± 0.002–0.005 mm and a surface roughness of Ra 0.2–0.4 µm are achieved. A starting hole is required for closed internal profiles;
  • Plunging: The electrode, made of copper or graphite, has the negative shape of the cavity and is slowly lowered into the workpiece, which is immersed in oil. This process is used to create mold cavities, blind cavities with sharp corners, deep, thin ribs, and raised lettering in molds. The electrode is made slightly smaller than the cavity on each side and wears down a bit as well; a new one is used for the finishing process.
± Vwire (Ø 0.1–0.3 mm)upper guidelower guideworkpieceWire (in deionized water)electrode(copper or graphite)dielectric oilworkpiecegapPlunging
Figure 23.14 · On the left, the wire stretched between the two guides cuts through the workpiece; the power supply provides the voltage between the wire and the workpiece. On the right, the shaped electrode descends into the workpiece submerged in oil, always maintaining a gap.

The wire cutting speed is given in mm² per minute: this is the area of the cut wall, that is, the length of the profile multiplied by the height of the workpiece. A modern machine performing roughing on steel achieves a rate of 100 to 300 mm²/min; finishing passes are much faster in length, because they remove only a few hundredths.

Flush-Cut Time and Thread Compensation
t = L · HvA offset = dthread2 + gap
t time in minutes · L Profile length in mm · H Workpiece height in mm · vA cutting speed in mm²/min · offset distance between the center of the wire and the desired contour, in mm (on the CNC, this is the radius compensation, G41/G42, as with a milling cutter) · dthread wire diameter · gap discharge gap, from 0.02 to 0.05 mm
Example 23.19 · A wire-cut die and a plunge electrode

Cut a 40-mm-high hardened steel die with a 180-mm-long profile flush with the edge. Roughing is performed at 120 mm²/min using a Ø0.25 wire and a gap of 0.03 mm; followed by two finishing passes at 9 mm/min.

Cut area: 180 × 40 = 7,200 mm² → roughing: 7,200 / 120 = 60 min (i.e., 120 / 40 = 3 mm/min along the profile)
Review: 2 · 180 / 9 = 40 min → total 100 min
Roughing offset: 0.25 / 2 + 0.03 = 0.155 mm; groove width approximately 2 × 0.155 = 0.31 mm

For the same matrix, you will also need a 20 × 30 mm rectangular blind countersink with a 0.1 mm gap on each side.

electrode: (20 − 2 × 0.1) × (30 − 2 × 0.1) = 19.8 × 29.8 mm
Approximately 1 hour and 40 minutes of file; offset 0.155 mm; stick electrode 19.8 × 29.8 mm
ProcessMaterialsThicknessesGrooveAccuracyWhen It's Worth It
Fiber lasermetals, including reflective ones; plastics, woodsteel up to 25–30 mm0.1–0.4 mm± 0.05–0.1 mmthin and medium-gauge sheet metal, precision profiles, series
Plasmaconductive metalsup to 30–50 mm1.5–4 mm± 0.3–0.5 mmmetal fabrication, medium thicknesses, low cost
Oxy-cuttingonly carbon steels and low-alloy steelsfrom 3 to over 300 mm1–5 mm± 0.5–1 mmthick sheets, construction site
Water Jetany materialup to 100–200 mm0.8–1.2 mm± 0.1 mmheat-sensitive materials, composites, glass, stone
Wire Electrical Discharge Machiningonly conductors, including hardened onesup to 300–400 mm0.15–0.4 mm± 0.002–0.005 mmdies, punches, molds, precision-hardened workpieces
Die-sinking EDMonly conductors, including hardened onesdeep cavitiesgap 0.05–0.3 mm± 0.005–0.01 mmmold marks, blind holes, sharp corners

Guideline values for comparing processes, compiled by us.

23.14 Additive Manufacturing

Additive manufacturing, or 3D printing, builds a workpiece layer by layer based on a CAD model, which a program (the slicer) divides into thin slices. No molds or tools are needed, and it is possible to create shapes that are impossible to produce using other machining operations: lightweight lattice structures, curved internal channels, and one-of-a-kind custom workpieces. Chapter 21 has already presented the techniques for polymers from a materials perspective; here, we compare them with those for metals.

  • FDM (fused filament deposition): A thermoplastic filament passes through a heated nozzle and is extruded in thin strands, layer by layer. Affordable machines, engineering plastics (PETG, ABS, fiber-reinforced polyamides), sturdy workpieces but with clearly visible layers;
  • SLA (stereolithography): Ultraviolet light cures a liquid resin, layer by layer. Extremely fine details and smooth surfaces: models, aesthetic prototypes, masters for lost-wax casting;
  • SLS (laser sintering of plastic powders): A laser fuses the granules of a polyamide powder laid down in layers. The powder that has not been fused provides structural support for the workpiece, so no supports are needed: functional workpieces, even in small batches;
  • Laser metal fusion (LPBF, Laser Powder Bed Fusion, also known as SLM): similar to SLS, but the powder is metallic (316L stainless steel, maraging steel, Ti6Al4V titanium, AlSi10Mg aluminum, nickel superalloys) and the laser completely melts it in an argon atmosphere. The resulting workpieces are nearly 100% dense, with strength similar to that of castings or rolled materials. Support structures are required to support overhanging workpieces and dissipate heat.
printing platematerial threadprint head and hot nozzlehlayersdesired surfacesteph
Figure 23.15 · On the left, FDM printing: the nozzle deposits one bead after another, and the workpiece grows one layer h at a time. On the right, a sloped surface becomes a staircase with steps h high: this is the step effect.

Strengths and Limitations

Advantages: freedom of form, no special equipment required, very little material waste (especially for titanium and superalloys, which are extremely expensive), short lead times from drawings to finished workpieces, and the ability to combine multiple parts into a single workpiece. Limitations: it is slow and expensive for mass production; the workpieces are anisotropic (weaker between layers); there are internal stresses and heat-induced deformations, the maximum size is limited by the machine’s chamber, and, above all, the surface is rough and the precision is insufficient for fits. Sloped surfaces exhibit a step-like effect: the thinner the layer, the smoother the workpiece, but more layers are needed, and the process takes longer.

TechniqueMaterialsLayerTypical Ra (µm)Accuracy
FDMFilled PLA, PETG, ABS, PA0.1–0.3 mm10-25± 0.2–0.5 mm
ALSphotopolymer resins0.025–0.1 mm1-3± 0.05–0.15 mm
SLSPA12, PA110.1–0.12 mm6-12± 0.2–0.3 mm
Laser Melting of Metalsstainless steel, maraging steel, titanium, aluminum, superalloys0.02–0.06 mm6-15± 0.05–0.2 mm

These are approximate values, compiled by us: they vary significantly depending on the machine, the orientation of the workpiece, and the parameters.

After Printing: Machine Tools

A stamped metal workpiece is not finished. The typical process is: relaxation back in the oven on the platform (to relieve stress), break from the platform using wire EDM or a band saw, removal of the supports, sometimes hot isostatic pressing (HIP) to seal the pores, then machine tool machining functional surfaces: calibrated holes, bearing seats, threads, and bearing surfaces. For this reason, in the model to be printed, the following are left allowance for excess metals 0.3–1 mm on those surfaces, as in a cast part, and support structures and reference points are provided for machine clamping. Additive manufacturing and material removal are not rivals: they work together.

Example 23.20 · How long does a metal print take?

A maraging steel mold insert is 60 mm tall. It is printed using laser sintering in 0.04 mm layers; between the application of powder and the laser pass, each layer takes an average of 40 seconds. The Ø20 H7 hole in the workpiece is printed at Ø19 and then reamed.

number of layers: 60 / 0.04 = 1,500
time: 1500 · 40 = 60,000 s = 60,000 / 3,600 = 16.7 h, or about 16 hours and 40 minutes
allowance around the hole: (20 − 19) / 2 = 0.5 mm per side
Using FDM with 0.2 mm layers, the same workpiece (made of plastic, as a prototype) would have 60 / 0.2 = 300 layers
1,500 layers and nearly 17 hours of machining, plus the expansion, removal, and boring of the hole
🖥️
From the blank to the finished part. Castings, molded workpieces, laser-cut workpieces, and 3D-printed workpieces almost always end up on machine tools for finishing. In the CNC Code simulator, you can start with a blank that isn’t a round bar and test the finishing program without risking a workpiece that has already cost money in foundry work, tooling, or printing hours.

11:15 p.m. The formulas in this chapter

What Are You Looking For?FormulaUnits
Dimensions of the Foundry ModelLm = Lg · (1 + r / 100)mm
Expansion Due to Warpinge = h · tan αmm
Recrystallization temperatureTr ≈ 0.4 · Tf (in kelvin)K
Percentage Reductionε = (h0 − h1) / h0 · 100%
Lamination, constant volumeL1 = L0 · h0 / h1 · v1 = v0 · h0 / h1mm · m/s
Maximum reduction for passesΔhmax ≈ μ² · Rmm
Extrusion RatioR = A0 / A1 · L1 = L0 · Rpure number · mm
Drawing passesn = ln (A0 / An) / ln (1 / (1 − q))number
Shearing ForceF = p · s · τR · τR ≈ 0,8 · RmN
Shearing OperationsW = λ · F · s (λ ≈ 0,5)N·mm
Play on the wingg = c · s · punch = D − 2g (shearing) · die = d + 2g (punching)mm
Development of a 90° bendarc = π/2 · (r + K · s) · straight segment = outer side − (r + s)mm
Bending Force in AirF ≈ 1,33 · L · s² · Rm / VN
Disc for a cylindrical glassD = √(d² + 4 · d · h) · β = D / dmm
Round bar for rolled filletsdtondo ≈ d − 0.6495 · Pmm
Porosity of a Sintered MaterialP = (1 − ρ / ρfull) · 100%
Laser Cutting Timet = L / v + n · tsfmin
Wire EDM processing timet = L · H / vA · offset = wire diameter / 2 + gapmin · mm
Layers of a 3D printN = H / h · t = N · t_layernumber · s

23.16 Exercises

Try to solve them on your own, using a calculator, before looking at the answers. The material data are the same as those given in the chapter.

Exercise 1. An aluminum alloy casting must be 250 mm long. How long must the pattern be, given a shrinkage of 1.3%?
Solution

Lm = 250 × 1.013 = 253.25 mm.

Exercise 2. A mold is 505 mm long, and the resulting casting measures 500 mm. What is the amount of shrinkage? What metal is the casting likely made of?
Solution

1 + r / 100 = 505 / 500 = 1.01, so r = 1%: this is the typical shrinkage of gray cast iron.

Exercise 3. Zinc melts at 419.5 °C. Estimate its recrystallization temperature: Is a sheet of zinc bent at 20 °C formed through hot or cold working?
Solution

Tr ≈ 0.4 · (419.5 + 273.15) = 0.4 · 692.65 = 277.1 K = 3.9 °C. At 20 °C, the temperature is above Tr: the machining is, at the very limit, hot working, and in fact, zinc work-hardens very little at room temperature.

Exercise 4. A sheet of metal 2.5 mm thick and 800 mm long is cold-rolled to a thickness of 1.5 mm without expanding in width. What is its final length, and what is the percentage reduction?
Solution

L1 = 800 × 2.5 / 1.5 = 1333.3 mm; reduction = (2.5 − 1.5) / 2.5 × 100 = 40%.

Exercise 5. A billet with a diameter of 150 and a length of 500 mm is extruded into a profile with a cross-sectional area of 900 mm². Find the extrusion ratio and the length of the profile, neglecting the end caps.
Solution

A0 = π · 150² / 4 = 17,671 mm²; R = 17,671 / 900 = 19.63; L1 = 500 · 19.63 = 9,817 mm, approximately 9.8 m.

Exercise 6. A 40 × 40 mm square is cut from a 1.5 mm-thick stainless steel sheet with Rm = 600 N/mm². What force is required?
Solution

p = 4 × 40 = 160 mm; τR = 0.8 × 600 = 480 N/mm²; F = 160 × 1.5 × 480 = 115,200 N, approximately 115 kN.

Exercise 7. A Ø12 hole is punched in a 4 mm-thick sheet of mild steel with a 6% clearance on each side. What are the diameters of the punch and die?
Solution

g = 0.06 × 4 = 0.24 mm. In punching, the punch has a hole diameter of Ø12; the die is 12 + 2 × 0.24 = Ø12.48.

Exercise 8. A bent angle bar has outer sides measuring 40 and 40 mm, a thickness of 2 mm, and an inner radius of 2 mm. Calculate its net area.
Solution

r / s = 1 → K = 0.33. Straight segments: 40 − (2 + 2) = 36 mm each. Arc: π / 2 · (2 + 0.33 · 2) = 1.5708 · 2.66 = 4.18 mm. L = 36 + 36 + 4.18 = 76.18 mm.

Exercise 9. A sheet of metal 1.5 m long and 2 mm thick, with Rm = 400 N/mm², is bent in air using a die with V = 16 mm. What force is required?
Solution

F = 1.33 × 1,500 × 2² × 400 / 16 = 199,500 N, approximately 200 kN, or 199,500 / 9,810 = 20.3 t.

Exercise 10. A glass with a diameter of 50 and a height of 80 mm is to be deep-drawn. Calculate the starting disc. Can this be done in a single operation with a limit β of 2.0? If not, how many operations are needed with re-drawing ratios of 1.25?
Solution

D = √(50² + 4 × 50 × 80) = √(2,500 + 16,000) = √18,500 = 136.0 mm; β = 136.0 / 50 = 2.72 > 2.0: one operation is not sufficient. First deep drawing to 136.0 / 2.0 = 68.0 mm; second deep drawing to 68.0 / 1.25 = 54.4 mm; the third reaches Ø50 (ratio 54.4 / 50 = 1.09, less than 1.25). Three operations are required.

Exercise 11. What diameter should the round bar be prepared to roll M8 × 1.25 screws?
Solution

d2 = 8 − 0.6495 × 1.25 = 8 − 0.812 = 7.188 mm: round bar with a diameter of approximately Ø7.19.

Exercise 12. A 25-mm-tall hardened steel punch has a 240-mm-long profile. How long does it take to perform roughing on it at a feed rate of 150 mm²/min?
Solution

Area = 240 × 25 = 6,000 mm²; t = 6,000 / 150 = 40 min.

Exercise 13. A 30-mm-tall resin prototype is printed using SLA in 0.05-mm layers, with each layer taking 10 seconds. How many layers, and how long will it take?
Solution

N = 30 / 0.05 = 600 layers; t = 600 × 10 = 6,000 s = 100 min, or 1 hour and 40 minutes.